Polyimide fibrofelt prepreg, preparation method thereof, composite material and application

Through the hot rolling combination of polyimide fiber mat and modified resin, a lighter and more high-temperature resistant polyimide fiber mat prepreg is formed, which solves the problems of insufficient temperature resistance and weight in the existing technology. Achieved better composite processability and flame retardant properties.

CN118853005APending Publication Date: 2024-10-29JIANGSU XIANNUO NEW MATERIAL TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410863824.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing polyimide fiber prepregs have deficiencies in temperature resistance, weight and composite processability, and there is a lack of polyimide fiber mat prepregs.

Method used

The polyimide fiber felt is combined with thermosetting resin by hot rolling. Through modified resin such as modified bismuth resin or modified epoxy resin, ester bonds, ether bonds, imidazole, cyanamide, amino, urea and other groups are added. The group is formed into a resin film layer. It is preferable to add release paper and PE film, and control the weight between 15g/m2 and 200g/m2 to improve temperature resistance and processability.

Benefits of technology

A lighter and more high-temperature-resistant polyimide fiber mat prepreg has been realized, with a lower weight. The coating and composite process temperature can be between 80 and 120°C, and the temperature resistance can reach over 260°C, which improves the resistance. combustion performance and process performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118853005A_ABST
    Figure CN118853005A_ABST
Patent Text Reader

Abstract

The invention discloses a polyimide fiber felt prepreg and a preparation method thereof as well as a composite material and application thereof, the polyimide fiber felt prepreg comprises a polyimide fiber felt layer (1) and thermosetting resin adhesive film layers (2) on two sides of the polyimide fiber felt layer (1), and the thermosetting resin adhesive film layers (2) are combined with the polyimide fiber felt layer (1) in a hot rolling manner; the gram weight of the polyimide fiber felt prepreg is 15g / m < 2 >-200g / m < 2 >. A composite material product obtained by processing the fiber prepreg has the excellent properties of light weight, high temperature resistance, radiation resistance, flame retardance and the like, and can be widely applied to military products such as aerospace, naval vessels, ships, automobiles, medical instruments and the like, civil products and many other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-performance fibers, and in particular to a polyimide prepreg and a preparation method thereof. Background Art

[0002] In recent years, with the iteration and upgrading of modern industries such as new aerospace vehicles, national defense and military industry, marine industry, automobile manufacturing, new energy and sports equipment, there is an urgent need for materials with high specific strength, high specific modulus, corrosion resistance, high temperature resistance, impact resistance, fracture resistance, fatigue resistance and high strength and lightweight. This undoubtedly provides a broad application market and development potential for high-performance fiber-reinforced resin-based composites.

[0003] The existing sound insulation technology adopts the double resonance cavity method (for example, CN113700159A, a high temperature resistant sound insulation board) or the method of adding damping felt (for example, CN110685367A, a sound insulation board). The latest technology refers to a composite sound insulation board (for example, CN113715417A, a composite sound insulation board), in which the sound insulation damping felt is compounded on the surface of the wooden board by an adhesive, and the main component of the sound insulation damping felt is EPDM. Chinese patent application CN109534839A discloses a method for preparing a carbon fiber composite sound insulation board, which adopts a composite board made of carbon fiber chopped fibers, which has the advantages of good waterproof, fireproof, anti-aging, impact resistance, low energy consumption, environmental protection, and no pollution to the environment after disposal.

[0004] Existing fiber felt prepregs include carbon fiber felt prepregs (e.g., CN209869447U, a carbon fiber felt composite glass fiber knitted felt prepreg; CN111073218A, an environmentally friendly flame-retardant chopped carbon fiber felt prepreg and a preparation method thereof). The addition of carbon fiber felt prepregs reduces the weight of the subsequent composite board. In addition, Chinese patent application CN113801439A discloses a surface felt prepreg and a preparation method thereof, in which polyester fiber felt and acrylonitrile fiber felt are introduced and compounded with epoxy resin to form a fiber felt prepreg.

[0005] Chinese patent document CN104130548A discloses a polyimide fiber prepreg and its preparation method and application, wherein the polyimide fiber prepreg comprises 40-80% by weight of polyimide fiber and 20-60% by weight of resin. The polyimide fiber prepreg provided by the invention is a prepreg prepared by impregnation of polyimide long fiber or its fabric as reinforcing fiber with cyanate resin, epoxy resin, bismaleimide or benzoxazine resin.

[0006] The existing fiber mat prepreg has the disadvantages of insufficient temperature resistance, heavy weight, insufficient fireproof grade, etc. In addition, the existing polyimide fiber prepreg uses polyimide long fiber or its fabric as reinforcing fiber, and there is still room for improvement in weight reduction, high temperature resistance, coating and composite processing. In addition, no polyimide fiber mat prepreg is disclosed in the prior art. Summary of the invention

[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a polyimide fiber felt prepreg, which can fill the gaps in the prior art and, compared with the existing polyimide fiber prepreg, improves at least any one of weight reduction, high temperature resistance, coating and composite processability.

[0008] Another object of the present invention is to provide a method for preparing the polyimide fiber felt prepreg.

[0009] Another object of the present invention is to provide a composite material comprising the polyimide fiber mat prepreg.

[0010] According to the purpose of the present invention, the present invention provides a polyimide fiber felt prepreg, which comprises a polyimide fiber felt layer (1) and resin film layers (2) on both sides thereof, wherein the resin film layer (2) and the polyimide fiber felt layer (1) are combined by hot rolling; the gram weight of the polyimide fiber felt prepreg is 15g / m 2 ~200g / m 2 .

[0011] In the present invention, the polyimide fiber felt is used to improve the temperature resistance of the resin reinforcement, and a novel polyimide fiber felt prepreg is provided. Compared with the existing polyimide fiber prepreg, the polyimide fiber felt prepreg is lighter and more resistant to high temperatures.

[0012] In the present invention, the resin can be one or more high-temperature resistant thermosetting resins selected from epoxy resin, bismaleimide resin, and cyanate ester resin. Preferably, the resin can be modified by adding modifying substances containing groups such as ester bonds, ether bonds, imidazole, cyanamide, amino groups, urea, etc., so as to ensure flame retardant properties on the one hand and improve the processability of the resin and extend the storage period of the resin on the other hand.

[0013] In addition, the polyimide fiber felt prepreg prepared by the present invention can achieve a gram weight of 15 to 200 g / m 2 , preferably 15 to 100 g / m 2 , more preferably 15 to 80 g / m 2 , more preferably 15 to 40 g / m 2 .

[0014] Preferably, the polyimide fiber felt prepreg further comprises a release paper layer (3) and a PE film layer (4) coated on the outside of the resin film layer (2).

[0015] Preferably, the thickness of the resin film layer (2) is 10 μm to 30 μm.

[0016] Preferably, the polyimide fiber felt prepreg contains 20 to 80% by weight of the polyimide fiber felt and 20 to 80% by weight of the thermosetting resin.

[0017] In the present invention, the weight of the polyimide fiber felt used is selected according to actual needs and can be 10 g / m 2 ~100g / m 2 In order to achieve the purpose of weight reduction, 10g / m 2 ~40g / m 2 , more preferably 10g / m 2 ~35g / m 2 .

[0018] According to the present invention, by using polyimide fiber mat to prepare prepreg, the production of polyimide prepreg with lower gram weight can be achieved. Since the gram weight of the polyimide fiber mat can be controlled to 10 to 35 g / m 2 Therefore, according to the type of resin used, the weight of polyimide fiber mat prepreg can be controlled to 15-40g / m 2 .

[0019] The thermosetting resin may be selected from at least one of modified bismaleimide resin, modified epoxy resin and modified cyanate ester resin, preferably modified bismaleimide resin or modified epoxy resin, more preferably modified bismaleimide resin.

[0020] According to the present invention, by using modified bismaleimide resin to prepare prepreg, the production of polyimide prepreg with better processability can be achieved, the coating and composite process temperature can be achieved between 80 and 120°C, and the temperature resistance can reach 260°C.

[0021] According to the present invention, by using modified epoxy resin to prepare prepreg, the production of polyimide prepreg with better processability can be achieved, the coating and composite process temperature can be achieved between 80 and 120°C, and the temperature resistance can reach 200°C.

[0022] In a preferred embodiment of the present invention, the modified bismaleimide resin is a product prepared by heating and stirring 10 parts by weight of diallyl bisphenol A epoxy, 4.2 parts by weight of methylimidazole, 1 part by weight of dicyandiamide and 100 parts by weight of bismaleimide resin at 120°C; and / or

[0023] The modified epoxy resin is a product prepared by heating and stirring 100 parts by weight of high temperature epoxy resin, 10 parts by weight of aminophenol tetrafunctional epoxy resin, 4.2 parts by weight of methylimidazole and 3 parts by weight of urea at 100°C.

[0024] By adopting the modified bismaleimide resin or modified epoxy resin, the process performance of the resin can be improved without affecting the temperature resistance, which is beneficial to the production operation of prepreg.

[0025] In the present invention, the fiber felt can be a mixture of multiple fibers, for example, a mixed felt of polyimide and aramid fiber, a mixed felt of polyimide and polyphenylene sulfide (PPS), a mixed felt of polyimide and carbon fiber, etc., so that the polyimide fiber felt can be changed to a mixed felt of polyimide fiber and aramid fiber, a mixed felt of polyimide fiber and polyphenylene sulfide fiber, or a mixed felt of polyimide and carbon fiber.

[0026] Another object of the present invention is to provide a method for preparing a polyimide fiber felt prepreg, which comprises the following steps:

[0027] 1) Film coating process: coating the resin to obtain a resin film; 2) Composite process: hot rolling composite the resin film with polyimide fiber felt to obtain a polyimide fiber felt prepreg.

[0028] Preferably, the resin is a modified bismaleimide resin or a modified epoxy resin. In step 1), the resin is heated to obtain a fluidized resin, and the molten resin is evenly coated on a release paper using a laminating machine, and covered with a layer of PE film to obtain a resin laminating film roll; in step 2), a polyimide fiber felt is taken and compounded with two resin laminating films obtained in step 1) under the action of a hot pressing roller; the temperature of the coating step and the compounding step is between 80 and 120°C.

[0029] Another object of the present invention is to provide a composite material, which is prepared from the above-mentioned polyimide fiber felt prepreg.

[0030] The polyimide fiber felt prepreg and composite material of the present invention can be widely used in the field of military products or civilian products, including aerospace, ships and boats, automobiles, sports equipment and medical equipment, such as sound insulation boards.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) Using polyimide fiber mat to improve the temperature resistance of the reinforcement, and providing a new type of polyimide fiber mat prepreg;

[0033] (2) Compared with the existing polyimide fiber prepreg, the gram weight (surface density) of the polyimide fiber mat prepreg prepared by the present invention can be achieved in the range of 15 to 200 g / m 2 , lighter in weight, can bring obvious effects in the fields of high temperature resistance and weight reduction;

[0034] (3) The resin adopts one or more high temperature resistant resins such as epoxy resin, bismaleimide resin, polyimide resin and cyanate resin, and modifies them to ensure the flame retardant performance on the one hand and improve the processability of the resin on the other hand. The coating and composite process temperature can be achieved between 80 and 120°C, and the temperature resistance can reach above 200°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic structural diagram of the polyimide fiber felt prepreg of the present invention.

[0036] The markings in the above drawings are as follows: polyimide fiber felt layer 1, resin film layer 2, release paper layer 3, PE film layer 4. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0038] In the present invention, "parts" refer to parts by weight unless otherwise specified. In addition, the endpoints and any values ​​of the range disclosed in the present invention are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in the present invention.

[0039] In the following examples and comparative examples:

[0040] Polyimide fiber felt comes from Jiangsu Xiannuo New Material Technology Co., Ltd., with a gram weight of 10g / m 2 ;

[0041] Polyimide continuous fabric comes from Jiangsu Xiannuo New Material Technology Co., Ltd., with a gram weight of 40g / m 2 ;

[0042] BMI resin was purchased from Honghu Shuangma New Material Technology Co., Ltd., and high-temperature epoxy was purchased from Nanyang Wanshixing Chemical.

[0043] The gram weight test method is in accordance with GB / T 32788.6 (Prepreg performance test method Part 6: Determination of mass per unit area), and the resin content test method is in accordance with GB / T 32788.5 (Prepreg performance test method Part 5: Determination of resin content).

[0044] Preparation Examples 1 and 2 are used to prepare modified bismaleimide resin or modified epoxy resin.

[0045] Preparation Example 1: Preparation of modified bismaleimide resin

[0046] 10 parts of diallyl bisphenol A epoxy, 4.2 parts by weight of methylimidazole, 1 part of dicyandiamide and 100 parts of bismaleimide resin were heated and stirred at 120° C. to obtain modified bismaleimide resin A.

[0047] Preparation Example 2: Preparation of modified epoxy resin

[0048] 100 parts by weight of high temperature epoxy (mainly composed of succinic anhydride epoxy derivative and phthalic anhydride), 10 parts by weight of aminophenol tetrafunctional epoxy (as a high temperature diluent), 4.2 parts by weight of methylimidazole, and 3 parts by weight of urea are heated and stirred at 100°C to obtain modified epoxy resin B.

[0049] Examples 1 to 4 are used to illustrate the preparation of polyimide fiber felt prepreg. The structure of the prepared polyimide fiber felt prepreg is as follows: Figure 1 shown.

[0050] Embodiment 1:

[0051] The preparation method of polyimide fiber felt prepreg adopts a two-step hot melt method, firstly, a modified bismaleimide resin is used for coating, and then it is used for the composite process. In the coating process, 1000g of modified bismaleimide resin A is heated at 90°C to obtain a fluid bismaleimide resin, and a film laminating machine is used to evenly coat the molten resin on the release paper, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film roll with a thickness of 10μm.

[0052] In the laminating process, 10g / m 2 The fiber felt product is compounded with the film under the action of the hot pressing roller by the tension rod, flattening rod, etc., and finally the upper release paper layer is taken off by the upper paper taking-up device at the prepreg winding position, and a layer of PE film is covered. Among them, the modified bismaleimide resin A improves the process performance of the resin without affecting the temperature resistance by modifying the bismaleimide resin phase, which is beneficial to the production operation of prepreg.

[0053] The prepreg prepared under this condition has a gram weight of 17g / m 2, the resin mass fraction in the prepreg is 40%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 180-200°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 260°C.

[0054] Embodiment 2:

[0055] In contrast to Example 1, Example 2 changes the grammage of the adhesive film to achieve production of polyimide fiber felt prepregs with different resin contents.

[0056] The preparation method of polyimide fiber felt prepreg adopts a two-step hot melt method, firstly, a modified bismaleimide resin is used for coating, and then it is used for the composite process. In the coating process, 3000g of modified bismaleimide resin A is heated at 90°C to obtain a fluid bismaleimide resin, and a film laminating machine is used to evenly coat the molten resin on the release paper, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film with a thickness of 30μm.

[0057] In the laminating process, 10g / m 2 The fiber felt product is sequentially passed through the tension rod, flattening rod, etc. and the film is compounded under the action of the hot pressing roller. Among them, the modified bismaleimide resin A improves the process performance of the resin without affecting the temperature resistance by modifying the bismaleimide resin phase, which is beneficial to the production operation of prepreg.

[0058] The prepreg prepared under this condition has a gram weight of 50g / m 2 , the resin mass fraction in the prepreg is 80%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 180-200°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 260°C.

[0059] Embodiment 3:

[0060] In Example 3, compared with Example 1, the grammage of the fiber mat is changed, so that the production of polyimide fiber mat prepregs with different grammages can be achieved.

[0061] The preparation method of polyimide fiber felt prepreg adopts a two-step hot melt method, firstly, a modified bismaleimide resin is used for coating, and then it is used for the composite process. In the coating process, 1000g of modified bismaleimide resin A is heated at 90°C to obtain a fluid bismaleimide resin, and a film laminating machine is used to evenly coat the molten resin on the release paper, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film with a thickness of 10μm.

[0062] In the laminating process, 100g / m 2The fiber felt product is sequentially passed through the tension rod, flattening rod, etc. and the film is compounded under the action of the hot pressing roller. Among them, the modified bismaleimide resin A improves the process performance of the resin without affecting the temperature resistance by modifying the bismaleimide resin phase, which is beneficial to the production operation of prepreg.

[0063] The prepreg prepared under this condition has a gram weight of 200g / m 2 , the resin mass fraction in the prepreg is 50%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 180-200°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 260°C.

[0064] Embodiment 4:

[0065] In contrast to Example 1, Example 4 changes the resin formula to achieve the production of polyimide fiber felt prepregs with different resin formulas.

[0066] The preparation method of polyimide fiber felt prepreg adopts a two-step hot melt method, firstly, a modified epoxy resin is used for coating, and then it is used for the composite process. In the coating process, 1000g of modified epoxy resin B is heated at 80°C to obtain a fluidized epoxy resin, and the molten resin is evenly coated on the release paper using a film laminating machine, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film with a thickness of 10μm.

[0067] In the laminating process, 10g / m 2 The fiber felt product is sequentially passed through the tension rod, flattening rod and the film is compounded under the action of the hot pressing roller. Among them, the modified epoxy resin B improves the process performance of the resin without affecting the temperature resistance by modifying the epoxy resin.

[0068] The prepreg prepared under this condition has a gram weight of 17g / m 2 , the resin mass fraction in the prepreg is 40%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 160-180°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 200°C.

[0069] Embodiment 5:

[0070] The preparation method of the mixed felt prepreg of polyimide fiber and aramid fiber adopts a two-step hot melt method, firstly, a modified bismaleimide resin is used for film coating, and then it is used for the composite process. In the film coating process, 1000g of modified bismaleimide resin A is heated at 90°C to obtain a fluid bismaleimide resin, and the molten resin is evenly coated on the release paper using a film laminating machine, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film roll with a thickness of 10μm.

[0071] In the laminating process, 10g / m 2 The mixed fiber felt product (of which aramid fiber accounts for 20 parts by weight and polyimide fiber accounts for 80 parts by weight) is compounded with the film under the action of the hot pressing roller through the tension rod, flattening rod, etc., and finally the upper release paper layer is taken off by the upper paper taking-up device at the prepreg winding position, and a layer of PE film is covered. Among them, the modified bismaleimide resin A improves the process performance of the resin without affecting the temperature resistance by modifying the bismaleimide resin phase, which is beneficial to the production operation of prepreg.

[0072] The prepreg prepared under this condition has a gram weight of 17g / m 2 The resin mass fraction in the prepreg is 40%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 180-200°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 240°C.

[0073] Embodiment 6:

[0074] The preparation method of the mixed felt prepreg of polyimide fiber and PPS fiber adopts a two-step hot melt method, firstly, a modified bismaleimide resin is used for film coating, and then it is used for the composite process. In the film coating process, 1000g of modified bismaleimide resin A is heated at 90°C to obtain a fluid bismaleimide resin, and the molten resin is evenly coated on the release paper using a film laminating machine, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film roll with a thickness of 10μm.

[0075] In the laminating process, 10g / m 2 The mixed fiber felt product (PPS fiber accounts for 60 parts by weight and polyimide fiber accounts for 40 parts by weight) is compounded with the film under the action of the hot pressing roller through the tension rod, flattening rod, etc., and finally the upper release paper layer is taken off by the upper paper taking-up device at the prepreg winding position, and a layer of PE film is covered. Among them, the modified bismaleimide resin A improves the process performance of the resin without affecting the temperature resistance by modifying the bismaleimide resin phase, which is beneficial to the production operation of prepreg.

[0076] The prepreg prepared under this condition has a gram weight of 17g / m 2 , the resin mass fraction in the prepreg is 40%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 180-200°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 260°C.

[0077] Embodiment 7:

[0078] The preparation method of the mixed felt prepreg of polyimide fiber and carbon fiber adopts a two-step hot melt method, firstly, a modified bismaleimide resin is used for coating, and then it is used for the composite process. In the coating process, 1000g of modified bismaleimide resin A is heated at 90°C to obtain a fluid bismaleimide resin, and the molten resin is evenly coated on the release paper using a film machine, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film roll with a thickness of 10μm.

[0079] In the laminating process, 10g / m 2 The mixed fiber felt product (of which carbon fiber accounts for 10 parts by weight and polyimide fiber accounts for 90 parts by weight) is compounded with the film under the action of the hot pressing roller through the tension rod, flattening rod, etc., and finally the upper release paper layer is taken off by the upper paper taking-up device at the prepreg winding position, and a layer of PE film is covered. Among them, the modified bismaleimide resin A improves the process performance of the resin without affecting the temperature resistance by modifying the bismaleimide resin phase, which is beneficial to the production operation of prepreg.

[0080] The prepreg prepared under this condition has a gram weight of 17g / m 2 , the resin mass fraction in the prepreg is 40%, the coating temperature of the resin is reduced to 80°C, the compounding temperature is 100°C, and the curing temperature is 180-200°C. The polyimide sheet prepared from this prepreg can withstand temperatures up to 260°C.

[0081] According to actual needs, the coating temperature and compounding temperature in the above embodiments 1 to 7 can be adjusted between 80 and 120° C. In addition, the mixing ratio of different fibers in the mixed fiber mats used in embodiments 5 to 7 can be adjusted according to actual needs and is not limited to the above embodiments.

[0082] Comparative Example 1:

[0083] Change the polyimide fiber felt to polyimide fabric (weight 40g / m 2 ), except for this, the preparation process is the same as that of Example 1 to prepare a polyimide fabric prepreg. The weight of the prepreg is 50 g / m 2 .

[0084] Comparative Example 2:

[0085] The preparation process was the same as that of Example 1 except that the bismaleimide resin A was changed to bismaleimide resin, and a polyimide fiber felt prepreg was prepared. When the bismaleimide resin was used, the processability was poor, the coating temperature was 150°C, and the compounding temperature was 170°C, which was not conducive to the production operation of the prepreg. In addition, the temperature resistance of the polyimide sheet prepared from the prepreg was lower than 250°C.

[0086] Comparative Example 3:

[0087] The epoxy resin B was changed to a high-temperature epoxy resin. The preparation process was the same as that of Example 4, and a polyimide fiber felt prepreg was prepared. When a high-temperature epoxy resin was used, the processability was poor, the coating temperature was 130°C, and the compounding temperature was 150°C, which was not conducive to the production operation of the prepreg. In addition, the temperature resistance of the polyimide sheet prepared from the prepreg was lower than 190°C.

[0088] From the comparison between Example 1 and Comparative Example 1, it can be seen that by using polyimide fiber felt to prepare prepreg, the production of polyimide prepreg with lower gram weight can be achieved. Since the gram weight of the polyimide fiber felt can be controlled to 10-35 g / m 2 Therefore, according to the type of resin used, the weight of polyimide fiber mat prepreg can be controlled to 15-40g / m 2 .

[0089] From the comparison between Example 1 and Comparative Example 2, it can be seen that by using modified bismaleimide resin to prepare prepreg, the production of polyimide prepreg with better processability can be achieved, the coating and composite process temperature can be achieved between 80 and 120°C, and the temperature resistance can reach 260°C.

[0090] From the comparison between the above-mentioned Example 4 and the comparative example 3, it can be seen that by using modified epoxy resin to prepare prepreg, the production of polyimide prepreg with better processability can be achieved, the coating and composite process temperature can be achieved between 80 and 120°C, and the temperature resistance can reach 200°C.

[0091] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A polyimide fiber felt prepreg, characterized in that: It comprises a polyimide fiber felt layer (1) and resin film layers (2) on both sides thereof, wherein the resin film layer (2) and the polyimide fiber felt layer (1) are combined by hot rolling; the polyimide fiber felt prepreg has a gram weight of 15 g / m 2 ~200g / m 2 .

2. The polyimide fiber mat prepreg according to claim 1, wherein: The polyimide fiber felt prepreg further comprises a release paper layer (3) and a PE film layer (4) coated on the outside of the resin film layer (2); and / or The thickness of the resin film layer (2) is 10 μm to 30 μm.

3. The polyimide fiber mat prepreg according to claim 1, wherein: The polyimide fiber felt prepreg comprises 20 to 80% by weight of polyimide fiber felt and 20 to 80% by weight of thermosetting resin; and / or The thermosetting resin is selected from at least one of modified bismaleimide resin, modified epoxy resin and modified cyanate ester resin; and / or The polyimide fiber felt has a gram weight of 10 g / m 2 ~100g / m 2 .

4. The polyimide fiber mat prepreg according to claim 3, wherein: The modified bismaleimide resin is a product prepared by heating and stirring 10 parts by weight of diallyl bisphenol A epoxy, 4.2 parts by weight of methylimidazole, 1 part by weight of dicyandiamide and 100 parts by weight of bismaleimide resin at 120° C.; and / or The modified epoxy resin is a product prepared by heating and stirring 100 parts by weight of high temperature epoxy resin, 10 parts by weight of aminophenol tetrafunctional epoxy resin, 4.2 parts by weight of methylimidazole and 3 parts by weight of urea at 100°C.

5. The polyimide fiber mat prepreg according to claim 3, wherein: The polyimide fiber felt prepreg has a gram weight of 15 to 100 g / m 2 , preferably 15 to 80 g / m 2 , more preferably 15 to 40 g / m 2 ; and / or The polyimide fiber felt has a gram weight of 10 g / m 2 ~40g / m 2 , preferably 10g / m 2 ~35g / m 2 .

6. The polyimide fiber mat prepreg according to claim 1, wherein: The polyimide fiber felt is changed to a mixed felt of polyimide fiber and aramid fiber, a mixed felt of polyimide fiber and polyphenylene sulfide fiber, or a mixed felt of polyimide fiber and carbon fiber.

7. A method for preparing a polyimide fiber mat prepreg according to any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: 1) Film coating process: coating the resin to obtain a resin film; 2) Composite process: subjecting the resin film and the polyimide fiber felt to a hot rolling composite process to obtain a polyimide fiber felt prepreg.

8. The preparation method according to claim 7, wherein: The resin is a modified bismaleimide resin or a modified epoxy resin. In step 1), the resin is heated to obtain a fluidized resin, the molten resin is evenly coated on a release paper using a film laminating machine, and then a layer of PE film is covered on the upper surface of the resin to obtain a resin film; In step 2), the polyimide fiber felt is compounded with the two resin films obtained in step 1) under the action of a hot pressing roller; The temperature of the coating step and the compounding step is between 80 and 120°C.

9. A composite material prepared from the polyimide fiber felt prepreg according to any one of claims 1 to 6.

10. Use of the polyimide fiber mat prepreg according to any one of claims 1 to 6 or the composite material according to claim 9 in the fields of aerospace, ships and vessels, automobiles, sports equipment and medical devices.

Citation Information

Patent Citations

  • Polyimide fiber prepreg and preparation method and application thereof

    CN104130548A

  • Preparation method of carbon fiber composite soundproof plate

    CN109534839A

  • Acoustic panel

    CN110685367A

  • Environment-friendly flame-retardant chopped carbon fiber felt prepreg and preparation method thereof

    CN111073218A

  • High-temperature-resistant sound insulation board

    CN113700159A