Long-service-life TPU color changing film and using method thereof

By using a combination of embossed bottom layer, acrylic pressure-sensitive adhesive layer, TPU color-changing layer and self-healing polyurethane resin layer in the car body color-changing film, the existing color-changing film's problems of easy delamination and yellowing are solved, and long life and weather resistance are achieved. The color-changing film has excellent physical properties and stability.

CN118853009AInactive Publication Date: 2024-10-29JIANGSU YAOSHENG NEW MATERIAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410987892.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing car body color-changing films are prone to delamination, yellowing and aging after use, resulting in a short service life.

Method used

It adopts a high-life TPU color-changing film composed of an embossed bottom layer, an acrylic pressure-sensitive adhesive layer, a TPU color-changing layer, a modified casting-grade material layer, a self-healing polyurethane resin layer and a gloss protective layer. It is prepared through specific heat treatment and composite processes to form Fusion of stacked layers and composite membranes to enhance the weather resistance and physical properties of the membrane.

Benefits of technology

It effectively avoids the delamination problem of the color-changing film, maintains the physical properties and stability, has good self-repairing effect, is not easy to yellow, has the characteristics of long life, strong weather resistance, long-lasting fit, no edge warping, no falling off, Removes no adhesive residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118853009A_ABST
    Figure CN118853009A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of color changing films, and provides a long-service-life TPU color changing film and a using method thereof. The TPU color-changing film sequentially comprises an embossing bottom layer, an acrylic pressure-sensitive adhesive layer, a TPU color-changing layer, a modified casting-grade material layer, a self-repairing polyurethane resin layer, a colloid scratch-resistant layer and a gloss protective layer from bottom to top. The preparation method of the TPU color-changing film comprises the following steps: S1, fusing the acrylic pressure-sensitive adhesive layer on the embossing bottom layer to obtain a coating layer A; s2, obtaining a fusion stacking layer B; s3, obtaining a composite film C; and S4, standing the composite film C obtained in the step S3 for 30-72 hours at the temperature of 35-70 DEG C, and rolling to obtain the long-service-life TPU color-changing film. The long-service-life TPU color-changing film disclosed by the invention effectively avoids the problem of delamination after color changing; meanwhile, the color-changing film contains the self-repairing polyurethane resin layer and is not prone to yellowing and aging, so that the color-changing film has the self-repairing effect and has the characteristic of long service life; in addition, the acrylic acid pressure-sensitive adhesive layer is contained, so that the adhesive tape has the characteristics of high weather resistance, long-acting adhesion, no edge warping, no falling off and no adhesive residue after being torn off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of color-changing films, and in particular relates to a long-life TPU color-changing film and a use method thereof. Background Art

[0002] Car body color-changing film is a service that uses a film with rich and diverse colors to change the appearance of the entire car or part of it by covering it with a whole layer. Car body color-changing film is mainly attached to the surface of the car body through polymer materials and is easy to remove. The mainstream car body color-changing film products in 2015 include: transparent film, automotive electroplating film, pearlescent film, glossy film, matte film, painted film, leather grain film, brushed film, electroplating film, electro-optical metal film, matte metal film (referred to as matte ice film).

[0003] In the prior art, there is, for example, a Chinese invention patent application that discloses a color-changing film with a publication number of CN115368838A, and the specific disclosed solution is "a color-changing film, composed from top to bottom of a release film layer, an installation adhesive layer, a color shielding layer, a color-changing layer, a TPU layer, a stain-resistant self-repairing layer, and a protective film layer". Although this color-changing film uses a stain-resistant self-repairing layer to effectively improve weather resistance and mechanical properties, achieve a self-repairing effect of the color-changing film, and extend its service life; however, due to the influence of the internal structure, it is prone to delamination after use, and is prone to yellowing and aging, resulting in a short service life. Summary of the invention

[0004] In view of the above problems existing in the prior art, an object of the present invention is to provide a long-life TPU color-changing film and a method for using the same.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A long-life TPU color-changing film, which is composed of an embossed bottom layer, an acrylic pressure-sensitive adhesive layer, a TPU color-changing layer, a modified casting-grade material layer, a self-repairing polyurethane resin layer, a colloid anti-scratch layer and a gloss protection layer from bottom to top. The preparation method of the TPU color-changing film comprises the following steps:

[0007] S1, coating the acrylic pressure-sensitive adhesive layer evenly on the upper and lower surfaces of the embossed bottom layer, and then placing the coated embossed bottom layer in an oven for heating time T of 3-8 hours, and setting the oven heating temperature to 70-150° C., so that the acrylic pressure-sensitive adhesive layer is fused to the embossed bottom layer to obtain a coating layer A;

[0008] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer, the TPU color-changing layer and the modified casting-grade material layer together to obtain a fused stacked layer B;

[0009] S3, coating the self-repairing polyurethane resin layer on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 1-2.8 μm; then adding a glue anti-scratch layer and a gloss protection layer for compounding to obtain a composite film C;

[0010] S4. Let the composite film C of step S3 stand at 35-70°C for 30-72h, then put it into a cooling machine and a winding device and wind it up to obtain a long-life TPU color-changing film.

[0011] As a preferred technical solution of the present invention, the TPU color-changing layer is calculated according to the weight parts of the following raw materials:

[0012] 70-100 parts of TPU thermoplastic polyurethane resin with a hardness value of 35-90A, 1-10 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, and 0-6 parts of filler.

[0013] As a preferred technical solution of the present invention, the TPU color-changing layer comprises 85 parts of TPU thermoplastic polyurethane resin with a hardness value of 80A, 5 parts of pigment, 4.5 parts of ultraviolet absorber, 3.5 parts of antioxidant stabilizer, and 2 parts of filler.

[0014] As a preferred technical solution of the present invention, the ultraviolet absorber includes at least one of benzotriazoles, diphenylacetones or hindered amines.

[0015] As a preferred technical solution of the present invention, the antioxidant stabilizer is a calcium zinc stabilizer or a phosphite.

[0016] As a preferred technical solution of the present invention, the filler is at least one of calcium carbonate, silicon dioxide, titanium dioxide and fluff powder.

[0017] As a preferred technical solution of the present invention, the self-repairing polyurethane resin layer is calculated according to the weight parts of the following raw materials:

[0018] 40-60 parts of isocyanate, 20-40 parts of polyol, 5-10 parts of chain extender, 2-5 parts of catalyst, 1-5 parts of anti-fouling agent, 10-15 parts of solvent, 1-5 parts of weather-resistant material and 1-3 parts of wetting agent.

[0019] As a preferred technical solution of the present invention, the anti-fouling auxiliary agent is acrylate functional group modified silicone oil.

[0020] As a preferred technical solution of the present invention, the wetting aid is a silicon-carbon structure polyether-modified polysiloxane. As a preferred technical solution of the present invention, the coupling agent is a silane coupling agent.

[0021] The present invention also provides a method for using the high-life TPU color-changing film as described above, comprising the following steps:

[0022] Step 1: Measure, clean and dry: Measure the size of the body where the adhesive needs to be pasted, then scrub and clean it with isopropyl alcohol, and then use drying equipment to dry it;

[0023] Step 2: Measure, cut and preheat: Measure the size of the long-life TPU color-changing film described in claims 1-9 and cut it, and use a heat gun to preheat the TPU color-changing film for a period of time T2 ranging from 0.3 to 0.6 hours;

[0024] Step 3: Film pasting: fix one end of the long-life TPU color-changing film, and then use a scraping tool to scrape and paste the other end of the TPU color-changing film, and tear off the bottom paper made of the embossed bottom layer at the same time; if there are bubbles or wrinkles, use a rag to wipe them repeatedly until the bubbles or wrinkles disappear;

[0025] Trimming and finishing: After applying the film, use a blade to cut off the excess TPU color-changing film, and use a heat gun to reinforce the edges, and you're done.

[0026] The present invention relates to a long-life TPU color-changing film and a method for using the same, which have the following beneficial effects: the long-life TPU color-changing film of the present invention contains a TPU color-changing layer, which can effectively avoid the problem of delamination after color change, and has excellent physical properties and stability; at the same time, it contains a self-repairing polyurethane resin layer, which is not easy to yellow and age, so that the self-repairing effect of the color-changing film has the characteristics of high life; in addition, it contains an acrylic pressure-sensitive adhesive layer, which has the characteristics of strong weather resistance, long-term adhesion, no warping, no falling off, and no residual glue after tearing off.

[0027] The present invention will be further described below in conjunction with specific implementation modes. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the structure of the high-life TPU color-changing film applied for by the present invention;

[0029] Figure 2 A flow chart of the method for using the long-life TPU color-changing film applied for by the present invention.

[0030] Reference numerals - In the drawings:

[0031] a-embossed base layer; b-acrylic pressure-sensitive adhesive layer; c-TPU color-changing layer; d-modified casting grade material layer; e-self-repairing polyurethane resin layer; f-colloidal anti-scratch layer; g-gloss protective layer. DETAILED DESCRIPTION

[0032] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0033] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplicity and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the present invention provides various specific examples of processes and materials, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.

[0034] Example 1

[0035] Raw materials - the TPU color-changing layer is calculated according to the weight parts of the following raw materials:

[0036] 74 parts of TPU thermoplastic polyurethane resin with a hardness value of 35A, 10 parts of pigment, 5 parts of ultraviolet absorber, 5 parts of antioxidant stabilizer, and 6 parts of filler.

[0037] The self-healing polyurethane resin layer applied for in the present invention is calculated according to the weight parts of the following raw materials: 50 parts of isocyanate, 20 parts of polyol, 8 parts of chain extender, 5 parts of catalyst, 5 parts of anti-fouling agent, 10 parts of solvent, 1 part of weather-resistant material and 1 part of wetting agent.

[0038] Please combine Figure 1 and Figure 2 As shown, the present invention provides a long-life TPU color-changing film, which is composed of an embossed bottom layer a, an acrylic pressure-sensitive adhesive layer b, a TPU color-changing layer c, a modified casting-grade material layer d, a self-repairing polyurethane resin layer e, a colloid anti-scratch layer f and a gloss protection layer g from bottom to top. The preparation method of the TPU color-changing film includes the following steps:

[0039] S1, coating the acrylic pressure-sensitive adhesive layer b evenly on the upper and lower surfaces of the embossed bottom layer a, and then placing the coated embossed bottom layer a in an oven for heating time T of 3h (preferably 3-8h), and setting the oven heating temperature to 110°C (preferably 70-150°C), so that the acrylic pressure-sensitive adhesive layer b is fused to the embossed bottom layer a to obtain a coating layer A;

[0040] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer a, the TPU color-changing layer c and the modified casting-grade material layer d together to obtain a fused stacked layer B;

[0041] S3, coating the self-repairing polyurethane resin layer e on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 1.2 μm (1-2.8 μm is preferred); then adding the anti-scratch glue layer f and the gloss protection layer g for compounding to obtain a composite film C;

[0042] S4. Place the composite film C of step S3 at a temperature of 35-70°C (35°C is preferred) for 30 hours (30-72 hours is preferred), and then place it in a cooling machine and a winding device and wind it up to obtain a high-life TPU color-changing film.

[0043] Example 2

[0044] Raw materials: 81 parts of TPU thermoplastic polyurethane resin with a hardness value of 38A, 5 parts of pigment, 5 parts of ultraviolet absorber, 5 parts of antioxidant stabilizer, and 4 parts of filler.

[0045] The self-healing polyurethane resin layer applied for in the present invention is calculated according to the weight parts of the following raw materials: 40 parts of isocyanate, 30 parts of polyol, 8 parts of chain extender, 5 parts of catalyst, 5 parts of anti-fouling agent, 10 parts of solvent, 1 part of weather-resistant material and 1 part of wetting agent.

[0046] Please combine Figure 1 and Figure 2 As shown, the present invention provides a long-life TPU color-changing film, which is composed of an embossed bottom layer a, an acrylic pressure-sensitive adhesive layer b, a TPU color-changing layer c, a modified casting-grade material layer d, a self-repairing polyurethane resin layer e, a colloid anti-scratch layer f and a gloss protection layer g from bottom to top. The preparation method of the TPU color-changing film includes the following steps:

[0047] S1. The acrylic pressure-sensitive adhesive layer is uniformly coated on the upper and lower surfaces of the embossed bottom layer, and then the coated embossed bottom layer a is placed in an oven for heating time T of 3.5 h (preferably 3-8 h), and the oven heating temperature is set to 120° C. (preferably 70-150° C.) to fuse the acrylic pressure-sensitive adhesive layer b to the embossed bottom layer a to obtain a coating layer A;

[0048] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer a, the TPU color-changing layer c and the modified casting-grade material layer d together to obtain a fused stacked layer B;

[0049] S3, coating the self-repairing polyurethane resin layer e on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 1.0 μm (1-2.8 μm is preferred); then adding the anti-scratch glue layer f and the gloss protection layer g for compounding to obtain a composite film C;

[0050] S4. Place the composite film C of step S3 at 36°C (35-70°C is preferred) for 34h (30-72h is preferred), and then place it in a cooling machine and a winding device and wind it up to obtain a high-life TPU color-changing film.

[0051] Example 3

[0052] Raw materials: 80 parts of TPU thermoplastic polyurethane resin with a hardness value of 60A, 9 parts of pigment, 4 parts of ultraviolet absorber, 4 parts of antioxidant stabilizer, and 3 parts of filler.

[0053] The self-healing polyurethane resin layer applied for in the present invention is calculated according to the weight parts of the following raw materials: 45 parts of isocyanate, 25 parts of polyol, 6 parts of chain extender, 5.2 parts of catalyst, 5.8 parts of anti-fouling agent, 9 parts of solvent, 2 parts of weather-resistant material and 2 parts of wetting agent.

[0054] Please combine Figure 1 and Figure 2 As shown, the present invention provides a long-life TPU color-changing film, which is composed of an embossed bottom layer a, an acrylic pressure-sensitive adhesive layer b, a TPU color-changing layer c, a modified casting-grade material layer d, a self-repairing polyurethane resin layer e, a colloid anti-scratch layer f and a gloss protection layer g from bottom to top. The preparation method of the TPU color-changing film includes the following steps:

[0055] S1, coating the acrylic pressure-sensitive adhesive layer b evenly on the upper and lower surfaces of the embossed bottom layer a, and then placing the coated embossed bottom layer a in an oven for a heating time T of 4 hours (preferably 3-8 hours), and setting the oven heating temperature to 120° C. (preferably 70-150° C.) to fuse the acrylic pressure-sensitive adhesive layer b to the embossed bottom layer to obtain a coating layer A;

[0056] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer a, the TPU color-changing layer c and the modified casting-grade material layer d together to obtain a fused stacked layer B;

[0057] S3, coating the self-repairing polyurethane resin layer e on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 1.5 μm (1-2.8 μm is preferred); then adding the anti-scratch glue layer f and the gloss protection layer g for compounding to obtain a composite film C;

[0058] S4. Place the composite film C of step S3 at 40°C (35-70°C is preferred) for 40h (30-72h is preferred), and then place it in a cooling machine and a winding device and wind it up to obtain a high-life TPU color-changing film.

[0059] Example 4

[0060] Raw materials: 85 parts of TPU thermoplastic polyurethane resin with a hardness value of 80A for the TPU color-changing layer, 5 parts of pigment, 4.5 parts of ultraviolet absorber, 3.5 parts of antioxidant stabilizer, and 2 parts of filler.

[0061] The self-healing polyurethane resin layer applied for in the present invention is calculated according to the weight parts of the following raw materials: 51 parts of isocyanate, 20 parts of polyol, 7 parts of chain extender, 5 parts of catalyst, 2 parts of anti-fouling agent, 10 parts of solvent, 2.5 parts of weather-resistant material and 2.5 parts of wetting agent.

[0062] Please combine Figure 1 and Figure 2 As shown, the present invention provides a long-life TPU color-changing film, which is composed of an embossed bottom layer a, an acrylic pressure-sensitive adhesive layer b, a TPU color-changing layer c, a modified casting-grade material layer d, a self-repairing polyurethane resin layer e, a colloid anti-scratch layer f and a gloss protection layer g from bottom to top. The preparation method of the TPU color-changing film includes the following steps:

[0063] S1, coating the acrylic pressure-sensitive adhesive layer b evenly on the upper and lower surfaces of the embossed bottom layer a, and then placing the coated embossed bottom layer a in an oven for a heating time T of 5 h (preferably 3-8 h), and setting the oven heating temperature to 120° C. (preferably 70-150° C.) to fuse the acrylic pressure-sensitive adhesive layer b to the embossed bottom layer to obtain a coating layer A;

[0064] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer a, the TPU color-changing layer c and the modified casting-grade material layer d together to obtain a fused stacked layer B;

[0065] S3, coating the self-repairing polyurethane resin layer e on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 2.0 μm (1-2.8 μm is preferred); then adding the anti-scratch glue layer f and the gloss protection layer g for compounding to obtain a composite film C;

[0066] S4. Place the composite film C of step S3 at 45°C (35-70°C is preferred) for 48h (30-72h is preferred), and then place it in a cooling machine and a winding device and wind it up to obtain a high-life TPU color-changing film.

[0067] Example 5

[0068] Raw materials: 90 parts of TPU thermoplastic polyurethane resin with a hardness value of 90A, 3 parts of pigment, 2 parts of ultraviolet absorber, 2.5 parts of antioxidant stabilizer, and 2.5 parts of filler.

[0069] The self-healing polyurethane resin layer applied for in the present invention is calculated according to the weight parts of the following raw materials: 50 parts of isocyanate, 20 parts of polyol, 5 parts of chain extender, 5 parts of catalyst, 4 parts of anti-fouling agent, 12 parts of solvent, 3 parts of weather-resistant material and 1 part of wetting agent.

[0070] Please combine Figure 1 and Figure 2 As shown, the present invention provides a long-life TPU color-changing film, which is composed of an embossed bottom layer a, an acrylic pressure-sensitive adhesive layer b, a TPU color-changing layer c, a modified casting-grade material layer d, a self-repairing polyurethane resin layer e, a colloid anti-scratch layer f and a gloss protection layer g from bottom to top. The preparation method of the TPU color-changing film includes the following steps:

[0071] S1. The acrylic pressure-sensitive adhesive layer is uniformly coated on the upper and lower surfaces of the embossed bottom layer, and then the coated embossed bottom layer is placed in an oven for heating time T of 8 hours (3-8 hours is preferred), and the oven heating temperature is set to 150° C. (70-150° C. is preferred) to fuse the acrylic pressure-sensitive adhesive layer to the embossed bottom layer to obtain a coating layer A;

[0072] S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer a, the TPU color-changing layer c and the modified casting-grade material layer d together to obtain a fused stacked layer B;

[0073] S3, coating the self-repairing polyurethane resin layer e on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 2.8 μm (1-2.8 μm is preferred); then adding the anti-scratch glue layer f and the gloss protection layer g for compounding to obtain a composite film C;

[0074] S4. Place the composite film C of step S3 at 70°C (35-70°C is preferred) for 72h (30-72h is preferred), and then place it in a cooling machine and a winding device and wind it up to obtain a high-life TPU color-changing film.

[0075] It should be noted that: in the above embodiments 1-5, the ultraviolet absorber includes at least one of benzotriazole, diphenylacetone or hindered amine; the antioxidant stabilizer is a calcium zinc stabilizer or a phosphite; the filler is at least one of calcium carbonate, silicon dioxide, titanium dioxide, and fluff powder; the antifouling agent is acrylate functional group modified silicone oil; the wetting agent is silicon carbon structure polyether modified polysiloxane. The technical parameters of silicon carbon structure polyether modified polysiloxane are as follows:

[0076] project index Element Polyether modified polysiloxane 1% surface tension dyn / cm 22 Solid content ≥90% color Colorless transparent liquid

[0077] This substance is produced by Tianchi Materials (Shenzhen) Co., Ltd., and its model is WETTINGAGENT28. The method of use of this product is: stir evenly before use, and disperse evenly after adding; usually 0.5% to 1.0% of the total amount, due to differences in formulas and selected raw materials, the specific amount of addition should be determined by experiments; store in a cool, ventilated place, and keep in a sealed container. The storage temperature is 3-40℃. If frozen, do not heat directly. It is better to melt at room temperature and then stir evenly before use.

[0078] Comparative Example 1

[0079] Different from Example 1, no TPU color-changing layer is provided during the preparation.

[0080] Comparative Example 2

[0081] Different from Example 1, no self-healing polyurethane resin layer is provided during the preparation.

[0082] Comparative Example 3

[0083] Different from Example 1, no acrylic pressure-sensitive adhesive layer is provided during the preparation.

[0084] Test example

[0085] Different from Example 1, no TPU color-changing layer, self-repairing polyurethane resin layer, and acrylic pressure-sensitive adhesive layer are provided during the preparation.

[0086] The corresponding performance tests were conducted on Examples 1-5, Comparative Examples 1-3 and Test Examples, wherein 9 Toyota Vezel cars were used as examples for the tests. The color-changing films of the above-mentioned Examples, Comparative Examples and Test Examples were attached by the same technician under the same environment, and the delamination, color change (observation of yellowing), tear strength (KN / m), residual glue after tearing, edge warping, etc. were recorded at different time periods of 1 day, 90 days, 180 days and 365 days. The data records for 1-90 days are shown in Table 1:

[0087]

[0088] The data records for 180 days are shown in Table 2:

[0089]

[0090] The data records for 365 days are shown in Table 3:

[0091]

[0092] From the above Tables 1-3, it can be seen that the TPU color-changing film embodiments 1-5 of the present invention have strong tear strength, and will not turn yellow or age after being used for a long time, will not delaminate, will not warp, and will not have residual glue during the tearing process; while the performance of the respective films of the test examples and comparative examples 1-3 in different time periods have obvious adverse phenomena, such as yellowing, delamination, low tear strength, etc.; the TPU used in the present invention is thermoplastic polyurethane, which is a polymer material with excellent elasticity and wear resistance, and the color-changing film utilizes the plasticity and colorability of TPU, by covering a thin layer on the surface of the substrate Film, thereby achieving the change of the original color; TPU color-changing film can not only maintain the texture and gloss of the original material, but also effectively resist the erosion of external factors such as ultraviolet rays and chemical corrosion, and extend the service life of the substrate; therefore, the TPU color-changing film obtained by the present invention application will not have the problem of delamination, and it has excellent physical properties and stability; at the same time, it contains a self-repairing polyurethane resin layer, which is not easy to yellow and age, so that the self-repairing effect of the color-changing film has the characteristics of high life; in addition, it contains an acrylic pressure-sensitive adhesive layer, which has strong weather resistance, long-term adhesion, and no warping, no falling off, and no residual glue after tearing off.

[0093] The present invention also provides a method for using the high-life TPU color-changing film as described above, comprising the following steps:

[0094] Step 1: Measure, clean and dry: Measure the size of the body where the sticker needs to be pasted, then use isopropyl alcohol to scrub and clean it, and then use drying equipment to dry it; the aforementioned scrubbing and cleaning with isopropyl alcohol can also be cleaned with a certain concentration of alcohol;

[0095] Step 2: Measure, cut and preheat: Measure the size of the long-life TPU color-changing film described in claims 1-9 and cut it, and use a heat gun to preheat the TPU color-changing film for a period of time T2 ranging from 0.3 to 0.6 hours; wherein T2 is preferably 2 hours;

[0096] Step 3: Film pasting: fix one end of the long-life TPU color-changing film, and then use a scraping tool to scrape and paste the other end of the TPU color-changing film, and tear off the bottom paper made of the embossed bottom layer at the same time; if there are bubbles or wrinkles, use a rag to wipe them repeatedly until the bubbles or wrinkles disappear;

[0097] Trimming and finishing: After applying the film, use a blade to cut off the excess TPU color-changing film, and use a heat gun to reinforce the edges, and you're done.

[0098] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0099] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A long-life TPU color-changing film, characterized in that: The TPU color-changing film is composed of an embossed bottom layer, an acrylic pressure-sensitive adhesive layer, a TPU color-changing layer, a modified casting-grade material layer, a self-repairing polyurethane resin layer, a colloid anti-scratch layer and a gloss protection layer from bottom to top. The preparation method of the TPU color-changing film includes the following steps: S1, coating the acrylic pressure-sensitive adhesive layer evenly on the upper and lower surfaces of the embossed bottom layer, and then placing the coated embossed bottom layer in an oven for heating time T of 3-8 hours, and setting the oven heating temperature to 70-150° C., so that the acrylic pressure-sensitive adhesive layer is fused to the embossed bottom layer to obtain a coating layer A; S2, heating the coating layer A obtained in step S1 at 120° C. to fuse and stack the embossed bottom layer, the TPU color-changing layer and the modified casting-grade material layer together to obtain a fused stacked layer B; S3, coating the self-repairing polyurethane resin layer on the surface of the fused stacking layer B obtained in step S2, wherein the dry glue thickness is set to 1-2.8 μm; then adding a glue anti-scratch layer and a gloss protection layer for compounding to obtain a composite film C; S4. Let the composite film C of step S3 stand at 35-70°C for 30-72h, then put it into a cooling machine and a winding device and wind it up to obtain a long-life TPU color-changing film.

2. A long-life TPU color-changing film as claimed in claim 1, characterized in that: The TPU color-changing layer is calculated based on the weight parts of the following raw materials: 70-100 parts of TPU thermoplastic polyurethane resin with a hardness value of 35-90A, 1-10 parts of pigment, 2-5 parts of ultraviolet absorber, 1-5 parts of antioxidant stabilizer, and 0-6 parts of filler.

3. A long-life TPU color-changing film as claimed in claim 2, characterized in that: The TPU color-changing layer comprises 85 parts of a TPU thermoplastic polyurethane resin having a hardness value of 80A, 5 parts of a pigment, 4.5 parts of an ultraviolet absorber, 3.5 parts of an antioxidant stabilizer, and 2 parts of a filler.

4. A long-life TPU color-changing film as claimed in claim 2, characterized in that: The ultraviolet absorber includes at least one of benzotriazoles, diphenylacetones or hindered amines.

5. A long-life TPU color-changing film as claimed in claim 2, characterized in that: The antioxidant stabilizer is a calcium zinc stabilizer or a phosphite.

6. A long-life TPU color-changing film as described in any one of claims 2 to 5, characterized in that: The filler is at least one of calcium carbonate, silicon dioxide, titanium dioxide and fluff powder.

7. A long-life TPU color-changing film according to any one of claims 1 to 5, characterized in that: The self-repairing polyurethane resin layer is calculated according to the weight parts of the following raw materials: 40-60 parts of isocyanate, 20-40 parts of polyol, 5-10 parts of chain extender, 2-5 parts of catalyst, 1-5 parts of anti-fouling agent, 10-15 parts of solvent, 1-5 parts of weather-resistant material and 1-3 parts of wetting agent.

8. A long-life TPU color-changing film as claimed in claim 7, characterized in that: The anti-fouling auxiliary agent is silicone oil modified with acrylate functional groups.

9. A long-life TPU color-changing film according to any one of claims 1 to 5, characterized in that: The wetting aid is silicon-carbon structure polyether modified polysiloxane.

10. A method for using the long-life TPU color-changing film according to any one of claims 1 to 9, characterized in that: The following steps are included Step 1: Measure, clean and dry: Measure the size of the body where the adhesive needs to be pasted, then scrub and clean it with isopropyl alcohol, and then use drying equipment to dry it; Step 2: Measure, cut and preheat: Measure the size of the long-life TPU color-changing film described in claims 1-9 and cut it, and use a heat gun to preheat the TPU color-changing film for a period of time T2 ranging from 0.3 to 0.6 hours; Step 3: Film pasting: fix one end of the long-life TPU color-changing film, then use a scraping tool to scrape and paste the other end of the TPU color-changing film, and tear off the base paper made of the embossed bottom layer at the same time; If there are bubbles or wrinkles, wipe them repeatedly with a rag until the bubbles or wrinkles disappear; Step 4: Trimming and finishing: After applying the film, use a blade to cut off the excess TPU color-changing film, and use a heat gun to reinforce the edges, and you are done.

Citation Information

Patent Citations

  • Embossing release film

    CN104999751A

  • Color changing film with self-repairing function and preparation method of color changing film

    CN109868073A

  • Color changing film

    CN115368838A

  • TPU color-changing film and preparation method thereof

    CN115895490A

  • Exterior film of building for protecting glass

    US20230398770A1