Silica gel conductive adhesive tape and application
By using silver-coated copper conductive powder and organic silica gel layer in conductive tape, combined with antistatic fluoroplastic release film, the problem of insufficient resistance of conductive tape in high and low temperature and chemical corrosive environments is solved, and stable adhesion in high temperature and high pressure environments is achieved. strength and safety for electronic devices.
Patent Information
- Application Number
- CN202411101610.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-29
AI Technical Summary
Existing conductive tapes show insufficient resistance under high and low temperature environments and chemical corrosion conditions, and have low silicon interface viscosity, making it difficult to meet the high communication quality requirements of electronic products.
The silicone conductive tape formed by using silver-coated copper conductive powder and organic silicone layer, combined with antistatic fluoroplastic release film, has a vertical impedance value of less than 0.004Ω/cm2 and has excellent temperature resistance, chemical corrosion resistance and wear resistance. , suitable for high temperature, high pressure and harsh environments.
Silicone conductive tape has stable adhesion at high temperatures of 300°C and low temperatures of -40°C. It is suitable for a wide range of electronic equipment applications, avoiding static electricity accumulation and discharge, and improving the durability and safety of the material.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive tapes, and in particular relates to a silicone conductive tape and an application thereof. Background Art
[0002] With the continuous development of the electronic products industry, people have higher and higher requirements for the communication quality of electronic products, so a large number of conductive tapes are being used more and more. The conductive tapes on the market are usually made by mixing conductive powder and pressure-sensitive adhesive, coating it on release paper, and then transferring it to metal foil and rolling it up, or mixing conductive powder and pressure-sensitive adhesive, coating it on release paper, and then transferring it to conductive cloth and rolling it up. Common conductive tapes on the market are usually not resistant to high and low temperatures, and have low adhesion to the silicon interface.
[0003] Therefore, in view of the above technical problems, it is necessary to provide a silicone conductive tape and its application.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide a silicone conductive tape and application thereof.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] Silicone conductive tape, including a release film and an organic silicone layer formed on the release film, the organic silicone layer including a coating layer and silver / copper conductive powder distributed in the coating layer, the silver / copper conductive powder is silver-coated copper particles, and its vertical impedance value is less than 0.004Ω / cm 2 .
[0008] In one or more embodiments of the present invention, the silver content in the silver / copper conductive powder is 3-5 wt %.
[0009] In one or more embodiments of the present invention, the particle size of the silver / copper conductive powder is not greater than 0.8 μm.
[0010] In one or more embodiments of the present invention, the silver / copper conductive powder is spherical particles.
[0011] In one or more embodiments of the present invention, the distribution amount of silver / copper conductive powder in the adhesive layer is 13-20 v / v%.
[0012] In one or more embodiments of the present invention, the thickness of the organic silicone layer is 10-80 μm.
[0013] In one or more embodiments of the present invention, the release film is an antistatic fluoroplastic release film, and at least a fluoro release layer is formed on the surface of the release film adjacent to the organic silicone layer.
[0014] In one or more embodiments of the present invention, the fluorine release layer is obtained by coating at least a fluorine release agent, which can be provided by Wuxi Longchi Fluorosilicone New Materials Co., Ltd.
[0015] In one or more embodiments of the present invention, the antistatic fluoroplastic release film includes an isolation layer, an antistatic coating, a substrate layer, an adhesive layer, a high temperature resistant film layer, an antistatic layer and a fluoro release layer arranged in sequence, which can be realized using existing technologies.
[0016] In one or more embodiments of the present invention, the isolation layer is a fluorinated organosilicon layer. Fluorinated organosilicon can significantly improve the high temperature resistance, electrical insulation, flexibility and reduce the surface energy of the material by introducing fluorine atoms.
[0017] In one or more embodiments of the present invention, the antistatic coating is a conductive material and an antistatic agent. Conductive materials such as metal powder, carbon fiber or conductive polymer are added to the coating, which can effectively conduct static electricity and avoid static electricity accumulation. Antistatic agent is a chemical substance that can reduce the surface resistance of the material, which can effectively reduce the static electricity generated by friction, thereby preventing static electricity accumulation and discharge.
[0018] In one or more embodiments of the present invention, the substrate layer is a PET film with a light transmittance greater than 95% and a haze less than 1%. The present invention uses the above PET film to make the release film have higher transparency.
[0019] In one or more embodiments of the present invention, the adhesive layer is any one of a silicone layer, an acrylic layer, a pressure-sensitive layer and an OCA optical layer. The present invention has a good bonding effect by using the above adhesive layer.
[0020] In one or more embodiments of the present invention, the high temperature resistant film layer is any one of a high temperature resistant PET film, a high temperature resistant PC film and a high temperature resistant PMMA film. The high temperature resistant film has good high temperature resistance and can still be used normally at higher temperatures.
[0021] In one or more embodiments of the present invention, the antistatic layer is a polyol ester antistatic layer or a quaternary ammonium salt antistatic layer. By adopting the polyol ester antistatic layer or the quaternary ammonium salt antistatic layer, the antistatic effect is good, and the situation that the release film is easy to adsorb dust impurities can be effectively avoided, and the release film will not generate static electricity during use, reducing safety hazards. In order to achieve the best use effect of the present invention: the quaternary ammonium salt antistatic layer is any one of dodecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, stearyl dimethyl amyl ammonium chloride and trihydroxyethyl methyl quaternary ammonium methyl sulfate. When the above quaternary ammonium salt is used, the antistatic effect is best.
[0022] In one or more embodiments of the present invention, the fluorine release layer is a fluorosilicone release layer. By using the fluorosilicone release layer, a better release effect is achieved.
[0023] In one or more embodiments of the present invention, the silicone conductive tape is used in electronic devices.
[0024] Compared with the prior art, the silicone conductive tape and its application of the present invention have excellent characteristics of temperature resistance, chemical corrosion resistance, wear resistance, etc., and therefore are widely used in high temperature, high pressure, strong corrosion and harsh environments. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0026] Silver / copper conductive powder uses silver-coated copper conductive particle filler, which greatly reduces its resistance value. Its vertical impedance value is less than 0.004Ω / cm 2 The silver-clad copper structure avoids the problem of easy oxidation of copper powder and reduces the cost of using pure silver powder.
[0027] The silicone layer is coated with transparent and environmentally friendly organic silicone water. Organic silicone adhesive is an adhesive synthesized using organic silicone polymer compounds. It is mainly used for bonding and sealing materials. Due to its excellent heat resistance, chemical corrosion resistance, wear resistance and other characteristics, it is widely used in high temperature, high pressure, strong corrosion and harsh environments. Organic silicone adhesive has excellent bonding effect and can bond a variety of different materials. It is often used to bond metals, plastics, silicone, glass and other materials. For those materials that are difficult to bond with traditional glue, organic silicone adhesive can solve the problem well.
[0028] The antistatic fluoroplastic release film comprises an isolation layer, an antistatic coating, a substrate layer, an adhesive layer, a high temperature resistant film layer, an antistatic layer and a fluoro release layer which are arranged in sequence from bottom to top. The upper surface and the lower surface of the antistatic coating are respectively bonded to the lower surface of the substrate layer and the upper surface of the isolation layer. The upper surface of the substrate layer and the lower surface of the high temperature resistant film layer are bonded through the adhesive layer. The upper surface and the lower surface of the antistatic layer are respectively bonded to the lower surface of the fluoro release layer. The fluoroplastic release film layer is used to protect / isolate the silicone layer. Preferably, a transparent polyester film Polyethylene terephthalate (PET) with a thickness of 50μm±5μm is used, which is coated with a fluorine release agent on one side and bonded to the silicone surface, that is, the thickness of the fluoroplastic release film layer is 50μm±5μm.
[0029] The thickness of the silicone conductive tape of the present invention is between 10-80 μm, and the vertical impedance value is less than 0.004 Ω / cm 2 The adhesion at room temperature is 0.3-1.6kg / 25mm, the adhesion at high temperature is 0.3-1.6kg / 25mm, the adhesion at low temperature is 0.3-1.7kg / 25mm, the high temperature application is 300℃, the low temperature application is -40℃, and the adhesion and application test are not easy to lose adhesion.
[0030] The silver-coated copper particles of the silver / copper conductive powder, including but not limited to the following embodiments, are prepared by the following method: lysozyme is used as a pre-protective layer of the copper powder to prevent oxidation of the copper powder, and then lysozyme is used as a transition layer to in situ reduce silver ions on its surface to form a uniform silver shell layer, and then low-temperature heating treatment is performed to prepare the silver-coated copper particles.
[0031] The preparation of the silver-coated copper particles used in the following embodiments may include but is not limited to:
[0032] 1. Prepare a N-2-hydroxyethylpiperazine-N'-2-ethanesulfonic acid buffer solution with a concentration of 28-55 mmol / L tri(2-carboxyethyl)phosphine, adjust the pH to 4.3-6.5 with sodium hydroxide, and record it as solution A; weigh lysozyme powder and add it to the N-2-hydroxyethylpiperazine-N'-2-ethanesulfonic acid buffer to prepare an N-2-hydroxyethylpiperazine-N'-2-ethanesulfonic acid buffer solution with a concentration of 4-15 mg / mL lysozyme, adjust the pH to 6.5-7.5 with sodium hydroxide, and record it as solution B; mix solution A and solution B in equal volumes to obtain solution C;
[0033] 2. Weigh copper powder and solution C and mix them evenly, let them stand at room temperature to form a pre-protective film on the surface of the copper powder, then centrifuge, wash with deionized water, and dry to obtain pretreated copper powder;
[0034] 3. The silver ammonia solution, the sodium citrate solution and the polyvinyl pyrrolidone solution are stirred and mixed uniformly at room temperature to obtain a silver ammonia solution dispersion; then the silver ammonia solution dispersion is placed in an acoustic resonance mixing device, the pretreated copper powder is added, and vitamin C solution is added in batches after the first mixing in the acoustic resonance mixing device, and the second to fourth mixing is performed, and the silver ions on the surface of the pretreated copper powder are reduced to nano silver particles, taken out, centrifuged, washed with water, and dried to obtain primary silver-coated copper particles; and finally the primary silver-coated copper particles are dried to obtain the silver-coated copper particles.
[0035] The preparation of the organic silicone adhesive for the coating layer including but not limited to the following embodiments can be:
[0036] 5L three-necked flask, equipped with thermometer, reflux condenser and constant pressure dropping funnel, oil bath heating. Add 800g toluene and 650g pentafluorostyrene in turn, stir to dissolve, add 2.6g chloroplatinic acid catalyst under nitrogen protection. Turn on the heating, after heating to 80°C, add 510g methyldichlorosilane, add it in 30min, and control the dropping time to about 1 hour. After the dropwise addition, continue to keep warm for 2 hours. After the reaction is completed, evaporate the solvent and unreacted methyldichlorosilane, collect the 132°C fraction (3.75kPa) by reduced pressure distillation, and obtain 950g of pentafluorophenylethyldimethylchlorosilane. The product purity measured by gas chromatography is 96.6% and the yield is 90.9%.
[0037] In a 250 mL conical flask, 80 g of trimethyl monochlorosilane, 194 g of pentafluorophenethyl dimethyl chlorosilane and 630 g of ethyl orthosilicate were mixed evenly to obtain a mixed silane for later use.
[0038] A 500mL three-necked flask is equipped with a thermometer, a reflux condenser and a constant pressure dropping funnel, and heated in an oil bath. First, 80g of water and 50g of concentrated sulfuric acid are carefully and slowly typed into 500g of tetrahydrofuran. After heating the mixture to 70°C, the above-prepared mixed silane is slowly added dropwise, and the dropping time is controlled to be about 45min. After the addition, the reaction is continued to be kept warm for 6 hours. Stop the reaction, and the reaction liquid is first decompressed and distilled to remove the by-product ethanol and the solvent tetrahydrofuran. The distillation temperature is 60°C, the vacuum degree is 10mmHg, and distillation is performed until no liquid is distilled out. Toluene is extracted 3 times, and 300g of toluene is used each time. Combine the extracts and wash with distilled water 5 times, using 150g of distilled water each time. After washing, add 60g of anhydrous sodium sulfate and dry for 5 hours. Filter to remove the desiccant, and distill at a temperature of 80°C and a vacuum degree of 0.5mmHg to obtain 380g of a white loose solid product containing fluorophenyl silicone resin.
[0039] (2) Polycondensation reaction A 2L three-necked flask is equipped with a thermometer, a water separator, a reflux condenser, a constant pressure feeding funnel, and oil bath heating. 180g 107 glue and 160g toluene are added in sequence, the temperature is raised to 80°C with stirring, and 1.7g dibutyltin dilaurate (DBTL) is added. Nitrogen is passed through, and a solution of 1.2g dimethyldiethoxysilane dissolved in 20g toluene is added dropwise. The addition is completed within 30 minutes, and the reaction is kept warm for 3h. Then, a solution of 220g fluorophenyl silicone resin dissolved in 210g toluene is added, the temperature is raised to 110°C, and the reaction is refluxed and separated for 24h.
[0040] (3) Post-treatment: Add 12 g of hexamethyldisilazane and 4.6 g of isopropanol to the polycondensation product, and heat-keep and ripen for 5 h. After the reaction is completed, stop the reaction, cool and discharge the material to obtain a high temperature resistant pressure-sensitive adhesive. During the ripening process, a small amount of uncondensed silanol groups further react.
[0041] (4) Glue coating process: 200g toluene, 4g fluorophenyl silicone pressure-sensitive adhesive and 0.1g dibenzoyl peroxide (BPO) were added to a container in sequence, and after being stirred evenly, the obtained diluted glue solution was coated on the polyester film with a glue coating machine, and the thickness of the glue layer was controlled to be 0.05-0.06mm. After coating, it was dried at 90℃ for 2min, and then dried at 150℃ for 5min to solidify.
[0042] In the following embodiments, the release film adopts a commercially available antistatic fluoroplastic release film, which does not affect the innovation of the present invention.
[0043] Example 1
[0044] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 3wt%. The particle size of the silver / copper conductive powder is 0.8μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 20v / v%. The room temperature adhesion of the sample is 0.3kg / 25mm, the high temperature adhesion is 0.2kg / 25mm, the low temperature adhesion is 0.3kg / 25mm, the high temperature application is 300℃, the low temperature application is -40℃, and the adhesion and application test are not easy to lose adhesion.
[0045] Example 2
[0046] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 3wt%. The particle size of the silver / copper conductive powder is 0.8μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 20v / v%. The room temperature adhesion of the sample is 0.8kg / 25mm, the high temperature adhesion is 0.7kg / 25mm, and the low temperature adhesion is 0.6kg / 25mm. The high temperature application is 300℃, and the low temperature application is -40℃. The adhesion and application test are not easy to lose adhesion.
[0047] Example 3
[0048] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 4wt%. The particle size of the silver / copper conductive powder is 0.8μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 20v / v%. The room temperature adhesion of the sample is 1.6kg / 25mm, the high temperature adhesion is 1.6kg / 25mm, the low temperature adhesion is 1.7kg / 25mm, the high temperature application is 300℃, the low temperature application is -40℃, and the adhesion and application test are not easy to lose adhesion.
[0049] Example 4
[0050] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 5wt%. The particle size of the silver / copper conductive powder is 0.4μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 20v / v%. The room temperature adhesion of the sample is 0.9kg / 25mm, the high temperature adhesion is 0.8kg / 25mm, and the low temperature adhesion is 0.6kg / 25mm. The high temperature application is 300℃, and the low temperature application is -40℃. The adhesion and application test are not easy to lose adhesion.
[0051] Example 5
[0052] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 5wt%. The particle size of the silver / copper conductive powder is 0.3 μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 20v / v%. The room temperature adhesion of the sample is 1.1kg / 25mm, the high temperature adhesion is 0.8kg / 25mm, and the low temperature adhesion is 1.1kg / 25mm. The high temperature application is 300℃, and the low temperature application is -40℃. The adhesion and application test are not easy to lose adhesion.
[0053] Example 6
[0054] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 5wt%. The particle size of the silver / copper conductive powder is 0.1 μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 20v / v%. The room temperature adhesion of the sample is 1.5kg / 25mm, the high temperature adhesion is 1.4kg / 25mm, and the low temperature adhesion is 1.45kg / 25mm. The high temperature application is 300℃, and the low temperature application is -40℃. The adhesion and application test are not easy to lose adhesion.
[0055] Example 7
[0056] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 5wt%. The particle size of the silver / copper conductive powder is 0.8μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 13v / v%. The room temperature adhesion of the sample is 1.3kg / 25mm, the high temperature adhesion is 1.1kg / 25mm, and the low temperature adhesion is 1.2kg / 25mm. The high temperature application is 300℃, and the low temperature application is -40℃. The adhesion and application test are not easy to lose adhesion.
[0057] Example 8
[0058] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 5wt%. The particle size of the silver / copper conductive powder is 0.8μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 15v / v%. The room temperature adhesion of the sample is 0.6kg / 25mm, the high temperature adhesion is 0.6kg / 25mm, the low temperature adhesion is 0.5kg / 25mm, the high temperature application is 300℃, the low temperature application is -40℃, and the adhesion and application test are not easy to lose adhesion.
[0059] Example 9
[0060] The silicone conductive tape of the present embodiment includes a release film and an organic silicone layer formed on the release film. The organic silicone layer with a thickness of 10-80 μm includes a coating layer and silver / copper conductive powder distributed in the coating layer. The silver / copper conductive powder is silver-coated copper particles. The silver content in the silver / copper conductive powder is 5wt%. The particle size of the silver / copper conductive powder is 0.8μm, and its vertical impedance value is less than 0.004Ω / cm 2 The distribution amount of silver / copper conductive powder in the coating layer is 18v / v%. The room temperature adhesion of the sample is 0.4kg / 25mm, the high temperature adhesion is 0.36kg / 25mm, the low temperature adhesion is 0.3kg / 25mm, the high temperature application is 300℃, the low temperature application is -40℃, and the adhesion and application test are not easy to lose adhesion.
[0061] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any embodiment reference in a claim should not be considered as limiting the claim to which it relates.
[0062] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A silicone conductive tape, comprising a release film and an organic silicone layer formed on the release film, wherein the organic silicone layer comprises a coating layer and silver / copper conductive powder distributed in the coating layer, wherein the silver / copper conductive powder is silver-coated copper particles, and its vertical impedance value is less than 0.004Ω / cm 2 .
2. The silicone conductive tape according to claim 1, characterized in that: The silver content in the silver / copper conductive powder is 3-5wt%.
3. The silicone conductive tape according to claim 1, characterized in that: The particle size of the silver / copper conductive powder is no more than 0.8 μm.
4. The silicone conductive tape according to claim 1, characterized in that: The silver / copper conductive powder is spherical particles.
5. The silicone conductive tape according to claim 1, characterized in that: The distribution amount of the silver / copper conductive powder in the adhesive coating layer is 13-20 v / v%.
6. The silicone conductive tape according to claim 1, characterized in that: The thickness of the organic silica gel layer is 10-80 μm.
7. The silicone conductive tape according to claim 1, characterized in that: The release film is an antistatic fluorine plastic release film, and at least a fluorine release layer is formed on the surface of the release film adjacent to the organic silicone layer.
8. The silicone conductive tape according to claim 7, characterized in that: The fluorine release layer is obtained by coating at least a fluorine release agent.
9. The silicone conductive tape according to claim 7, characterized in that: The antistatic fluoroplastic release film comprises an isolation layer, an antistatic coating, a substrate layer, an adhesive layer, a high temperature resistant film layer, an antistatic layer and a fluoro release layer which are arranged in sequence.
10. Use of the silicone conductive tape according to any one of claims 1 to 9 in electronic equipment.