Laser softening method for 2000MPa-grade ultrahigh-strength steel
Through the combination of rectangular laser spot and temperature control mode, the problems of poor temperature control uniformity and high energy consumption in the local softening of 2000MPa ultra-high-strength steel are solved, achieving high-efficiency, low-energy consumption softening effects, and improving the sample hardness and tensile strength. strength.
Patent Information
- Application Number
- CN202410908216.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
AI Technical Summary
The existing technology has problems such as poor uniformity of temperature control, high energy consumption, poor hardness stability in the soft zone and wide heat-affected zone during the local softening process of 2000MPa grade ultra-high-strength steel, which results in high mold costs, difficult development and easy deformation of the sample. .
A rectangular laser spot is used for laser softening. The temperature is controlled from 200°C to Ac1. The scanning speed and power are adjusted according to the thickness of the sample. Combined with the temperature control mode or power mode, the cooling method is air cooling to ensure the consistency of the shape and performance of the soft zone.
It achieves high-efficiency, low-energy local softening, increases the hardness and tensile strength of the soft zone, reduces sample deformation, and provides laser softening process parameters and performance indicators for 2000MPa ultra-high-strength steel.
Smart Images

Figure CN118854020A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel processing, and specifically relates to a laser softening method for 2000MPa-level ultra-high strength steel. Background Art
[0002] In recent years, new energy vehicles have developed rapidly, and the proportion of ultra-high-strength steel samples used by automakers in new models has gradually increased. This is because the use of ultra-high-strength steel samples to replace traditional steel in the manufacture of white bodies can achieve higher strength while using less material thickness, and greatly enhance the collision performance of the car while achieving weight reduction. The body of the ultra-high-strength sample has higher strength and anti-deformation ability.
[0003] Ultra-high strength steel is a type of alloy steel used to manufacture structural parts that withstand high stress. Generally, the yield strength is greater than 1180MPa and the tensile strength is greater than 1380MPa. This type of steel generally has sufficient toughness and high specific strength and yield ratio, as well as good weldability and formability. According to the degree of alloying and microstructure, it can be divided into three categories: low alloy, medium alloy and high alloy ultra-high strength steel. In February 2018, a new generation of ultra-high strength steel based on coherent nano-precipitation strengthening was developed, which won the 2017 Top Ten Scientific Advances.
[0004] In order to obtain better collision performance, the strength of ultra-high-strength steel used by automobile companies is continuously increasing. At present, some car body specimens have applied 2000MPa ultra-high-strength steel, and its hardness generally exceeds 600HV. Such high hardness will require higher riveting die force during SPR riveting, and the rivets are easily bent and deformed.
[0005] To address the above difficulties, the industry can generally pre-drill holes in 2000MPa-grade ultra-high-strength steel samples before riveting; or reduce the hardness of the riveted area through local tempering, improve plasticity, and form a local soft area.
[0006] The softening technologies currently used are:
[0007] 1. Use mold soft zone technology to soften the entire area that needs to be softened during hot stamping. Use high-temperature molds to reduce the cooling rate, so that austenite is transformed into ferrite and pearlite structure to obtain a low hardness soft zone.
[0008] 2. Use induction heating and flame heating technology to heat and temper the softened area or the entire area of the ultra-high strength sample to obtain a low hardness soft area.
[0009] Laser heat treatment is to quickly scan the workpiece with a high-energy laser beam, so that the surface temperature of the irradiated metal or alloy rises to above the phase change point at a very fast speed. When the laser beam leaves the irradiated part, due to the heat conduction, the cold matrix is rapidly cooled and self-quenched to obtain a finer hardened layer structure, and the hardness is generally higher than the conventional quenching hardness. The workpiece deformation is very small during the treatment process, which is suitable for surface strengthening of certain workpieces or local parts of the workpiece that cannot be completed or difficult to achieve with other quenching technologies. Laser heat treatment has a high degree of automation, and the depth and area of the hardened layer are well controllable. This technology is mainly used to strengthen the surface of automotive parts or molds, improve their surface hardness, wear resistance, corrosion resistance, strength and high temperature performance, such as laser heat treatment of automobile engine cylinder bores, crankshafts, stamping dies, casting molds, etc. The laser heat treatment process is: pretreatment (surface cleaning and pre-setting of light-absorbing coating) laser quenching (determining the hardening model and quenching process parameters)-quality inspection (macro and micro inspection).
[0010] Laser heat treatment is a method of surface treatment of metals using a high-power density laser beam. It can achieve surface modification such as phase change hardening (also known as surface quenching, surface amorphization, surface remelting quenching), surface alloying, etc., and produce changes in surface composition, organization, and performance that cannot be achieved by large surface quenching. After laser treatment, the surface hardness of cast iron can reach HRC60 or above, and the surface hardness of medium-carbon and high-carbon carbon steel can reach HRC70 or above, thereby improving its wear resistance, fatigue resistance, corrosion resistance, oxidation resistance and other properties, and extending its service life. Compared with other traditional heat treatment processes such as high-frequency quenching, carburizing, nitriding, etc., laser heat treatment technology has the following characteristics:
[0011] 1. No need to use additional materials, only the surface structure of the treated material is changed. The modified layer after treatment has sufficient thickness, and the depth can be adjusted as needed, generally up to 0.1-0.8mm.
[0012] 2. The bonding strength between the treated layer and the substrate is high. There is a dense metallurgical bond between the modified layer treated by laser surface treatment and the substrate material, and the surface of the treated layer is a dense metallurgical structure with high hardness and wear resistance.
[0013] 3. The deformation of the processed parts is very small. Due to the high power density of the laser, the action time on the parts is very short (10 -2 -10 seconds), so the thermal deformation area and overall change of the parts are very small. Therefore, it is suitable for high-precision parts processing as the final processing procedure of materials and parts.
[0014] 4. Good processing flexibility and wide application. The flexible light guide system can arbitrarily guide the laser to the processing part, so that deep holes, inner holes, blind holes and grooves can be easily processed, and selective local processing can be performed. Summary of the invention
[0015] The disadvantages of the existing softening technology are as follows:
[0016] 1. Mold soft zone technology has high mold cost, difficult development, poor temperature control uniformity and high energy consumption. When the soft zone is small, it is greatly affected by heat transfer and has poor temperature stability. If a large area is softened, the strength of the sample itself will be lost.
[0017] Induction heating has certain requirements on the shape of the soft zone and is difficult to control temperature; flame heating technology has poor temperature uniformity; both have problems such as high energy consumption, complex tooling, poor uniformity of the soft zone, large heat-affected range, and easy deformation of the specimen.
[0018] In order to solve the above-mentioned technical problems, this application provides the following technical solutions:
[0019] The present invention provides a laser softening process for 2000MPa ultra-high strength steel with respect to local softening technology. The laser heating technology is used to solve the problems of poor temperature control uniformity, high energy consumption, poor hardness stability of the soft zone, and wide heat-affected zone in the existing local softening process, and a set of laser softening process parameters for 2000MPa ultra-high strength steel is provided.
[0020] The present invention provides a laser softening method for 2000MPa ultra-high strength steel, wherein the hardness of the 2000MPa ultra-high strength steel is 520-700HV and the tensile strength is 1700-2200MPa;
[0021] The laser softening method comprises the following steps:
[0022] S1: laser softening the softened area of the 2000MPa grade ultra-high strength steel to obtain laser softened ultra-high strength steel; before laser softening, the 2000MPa grade ultra-high strength steel is placed on a laser softening workbench, and a processing path and laser parameters are set according to a desired soft zone shape.
[0023] The laser softening process uses a rectangular laser spot, and the laser softening temperature is 200°C to A c1 , where A c1 It is the temperature at which austenite transformation begins in 2000MPa grade ultra-high strength steel; a rectangular spot is used for laser softening to make its energy distribution more uniform.
[0024] The laser scanning speed described in this process is 1-40mm / s, which is related to the thickness of the sample. The thicker the sample, the slower the scanning speed is required to ensure the consistency of the soft zone performance. When 0.8mm≤t<1mm, the laser scanning speed is ≤40mm / s; when 1mm≤t<1.6mm, the laser scanning speed is ≤25mm / s; when 1.6mm≤t<2mm, the laser scanning speed is ≤15mm / s; when 2mm≤t<5mm, the laser scanning speed is ≤10mm / s; where t is the thickness of 2000MPa grade ultra-high strength steel;
[0025] S2: Cooling the laser softened ultra-high strength steel to complete the laser softening method.
[0026] Preferably, in step S1, the length of the rectangular laser spot is 5-40 mm, and the width is 1-8 mm.
[0027] Preferably, in step S1, when the rectangular laser spots are overlapped and scanned, the overlap rate is 5-20%.
[0028] Preferably, in step S1, the defocusing amount of the laser softening is -10 mm to +20 mm.
[0029] Preferably, in step S1, during laser softening, the angle between the incident laser and the surface of the softening area is 45-90°.
[0030] Preferably, in step S1, the laser power of the laser softening is 100-6000W.
[0031] Furthermore, in step S1, the laser softening is controlled by a temperature control mode or a power mode; in the temperature control mode, the temperature of the laser softening is 200°C-A c1 , the A c1 It is the starting temperature of austenite transformation of 2000MPa grade ultra-high strength steel; in the power mode, the power of laser softening is 800-4000W.
[0032] Preferably, in step S2, the cooling method is air cooling.
[0033] The present invention also provides an ultra-high strength steel prepared by the laser softening method.
[0034] Preferably, the hardness of the softened area of the ultra-high strength steel is 310-500 HV, the tensile strength is 1000-1600 MPa, and the elongation is 5-12%.
[0035] The technical solution of the present invention has the following advantages over the prior art:
[0036] (1) The present invention uses laser as a heat source, and the processing process is simple and efficient, with low energy consumption and high energy utilization rate.
[0037] (2) The present invention provides laser softening process parameters and corresponding soft zone performance indicators for 2000MPa grade ultra-high strength steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Schematic diagram of laser scanning method.
[0039] Figure 2 This is the softening temperature-hardness curve of 2000MPa ultra-high strength steel. DETAILED DESCRIPTION
[0040] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0041] Example 1
[0042] (1) A 2000MPa grade ultra-high strength steel sample with a thickness of 2.0mm was placed on a laser softening workbench. The soft zone size was a 20*35mm rectangle. The soft zone processing path was set. The laser softening parameters were focal length 310mm, spot size 4*20mm, temperature 400℃, and scanning speed 10mm / s.
[0043] (2) Start the laser softening equipment, remove the sample after heating is completed, and allow it to air cool to obtain a 2000 MPa grade ultra-high strength steel sample with a local soft area.
[0044] Example 2
[0045] (1) A 2000MPa grade ultra-high strength steel sample with a thickness of 2.0mm was placed on a laser softening workbench. The soft zone size was a 20*35mm rectangle. The soft zone processing path was set. The laser softening parameters were focal length 310mm, spot size 4*20mm, temperature 400℃, and scanning speed 10mm / s.
[0046] (2) Start the laser softening equipment, remove the sample after heating is completed, and allow it to air cool to obtain a 2000 MPa grade ultra-high strength steel sample with a local soft area.
[0047] Example 3
[0048] (1) A 2000MPa grade ultra-high strength steel sample with a thickness of 2.0mm was placed on the laser softening workbench. The soft zone size was a 20*35mm rectangle. The soft zone processing path was set. The laser softening parameters were focal length 310mm, spot size 4*20mm, temperature 600℃, and scanning speed 10mm / s.
[0049] (2) Start the laser softening equipment, remove the sample after heating is completed, and allow it to air cool to obtain a 2000 MPa grade ultra-high strength steel sample with a local soft area.
[0050] Example 4
[0051] (1) A 2000MPa grade ultra-high strength steel sample with a thickness of 2.0mm was placed on the laser softening workbench. The soft zone size was a 20*35mm rectangle. The soft zone processing path was set. The laser softening parameters were focal length 310mm, spot size 4*20mm, temperature 800℃, and scanning speed 10mm / s.
[0052] (2) Start the laser softening equipment, remove the sample after heating is completed, and allow it to air cool to obtain a 2000 MPa grade ultra-high strength steel sample with a local soft area.
[0053] Effect evaluation 1
[0054] Table 1 Performance test of the softened area of ultra-high strength steel prepared by the laser softening method of each embodiment
[0055] Sample Soft zone hardness HV Tensile strength MPa Yield strength MPa Elongation after break % Example 1 478.6 1618 1482 5.60 Example 2 418.9 1383 1243 6.41 Example 3 344.4 1084 976 10.92
[0056] The key technical point of the present invention is that the raw material is 2000MPa grade ultra-high strength steel. The laser softening process is proposed for the first time for this material. The softening rate, softening temperature, softening power process range and soft zone performance of 2000MPa grade ultra-high strength steel under different sample thicknesses are summarized, and the obtained product has excellent application performance.
[0057] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A laser softening method for 2000MPa ultra-high strength steel. It is characterized in that The 2000MPa grade ultra-high strength steel has a hardness of 520-700HV and a tensile strength of 1700-2200MPa; The laser softening method comprises the following steps: S1: laser softening the softened area of the 2000 MPa grade ultra-high strength steel to obtain laser softened ultra-high strength steel; The laser softening process uses a rectangular laser spot, and the laser softening temperature is 200°C to A c1 , where A c1 The temperature at which austenite transformation begins in 2000MPa grade ultra-high strength steel; The laser scanning speed is 1-40mm / s; when 0.8mm≤t<1mm, the laser scanning speed is ≤40mm / s; when 1mm≤t<1.6mm, the laser scanning speed is ≤25mm / s; when 1.6mm≤t<2mm, the laser scanning speed is ≤15mm / s; when 2mm≤t<5mm, the laser scanning speed is ≤10mm / s; where t is the thickness of 2000MPa grade ultra-high strength steel; S2: Cooling the laser softened ultra-high strength steel to complete the laser softening method.
2. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 1, It is characterized in that In the step S1, the length of the rectangular laser spot is 5-40 mm, and the width is 1-8 mm.
3. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 1, It is characterized in that In the step S1, when the rectangular laser spots are overlapped and scanned, the overlap rate is 5-20%.
4. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 1, It is characterized in that In the step S1, the defocusing amount of the laser softening is -10 mm to +20 mm.
5. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 1, It is characterized in that In the step S1, during laser softening, the angle between the incident laser and the surface of the softening area is 45-90°.
6. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 1, It is characterized in that In the step S1, the laser power of the laser softening is 100-6000W.
7. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 6, It is characterized in that In the step S1, the laser softening is controlled by a temperature control mode or a power mode; in the power mode, the power of the laser softening is 800-4000W.
8. The laser softening method for 2000MPa grade ultra-high strength steel as claimed in claim 1, It is characterized in that In step S2, the cooling method is air cooling.
9. An ultra-high strength steel produced by the laser softening method according to any one of claims 1 to 8.
10. The ultra-high strength steel according to claim 9, It is characterized in that The ultra-high strength steel has a hardness of 310-500 HV in the softened region, a tensile strength of 1000-1600 MPa, and an elongation of 5-12%.