Economical H2S corrosion resistant coiled tubing steel and production method thereof

By rationally proportioning the chemical components in the coiled tubing and adopting specific processes, a uniform austenite grain structure is formed, which solves the problem of hydrogen-induced cracking caused by the segregation of the hard phase structure in the existing technology and achieves economical H2S corrosion resistance. improvement and production cost reduction.

CN118854166APending Publication Date: 2024-10-29武汉钢铁有限公司

Patent Information

Application Number
CN202411217213.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing coiled tubing has hard phase segregation in high-pressure, fatigue and H2S corrosion environments, leading to hydrogen-induced cracking, and the economical H2S corrosion resistance is insufficient.

Method used

Adopting specific chemical composition combinations and process treatments, including reasonable proportions of C, Si, Mn, Cr, Nb, Cu, Ni, Ca, Mg and other elements, and through RH treatment, heating, rolling, cooling and coiling processes Steps, control temperature and time parameters to form a uniform austenite grain structure and improve the material's resistance to H2S corrosion.

Benefits of technology

Economical H2S corrosion-resistant coiled tubing steel has been realized, which avoids cracking problems, improves the material's resistance to HIC and SSCC, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005021879290000061
    Figure BDA0005021879290000061
  • Figure BDA0005021879290000071
    Figure BDA0005021879290000071
  • Figure BDA0005021879290000072
    Figure BDA0005021879290000072
Patent Text Reader

Abstract

The invention relates to economical H2S corrosion-resistant coiled tubing steel, which comprises the following components in percentage by weight: 0.07 to 0.25 percent of C, less than or equal to 0.48 percent of Si, 0.33 to 1.28 percent of Mn, less than or equal to 0.016 percent of P, less than or equal to 0.0013 percent of S, 0.014 to 0.041 percent of Al, 0.008 to 0.057 percent of Nb, less than or equal to 0.0043 percent of N, less than or equal to 0.0023 percent of O, and any two or more but not including a mixture which is added at the same time in Cu, Ni, Cr, Mo, V, Ti and B, the production method comprises the following steps: continuously casting in batches after conventional smelting; heating the casting blank; rolling is conducted; cooling is performed; and coiling. The steel plate is relatively economical, the HIC corrosion resistance and the SSCC corrosion resistance of the steel plate are not cracked after being quenched and tempered, the qualification rate of the prepared coiled tubing is increased, the production cost is reduced, and the service life is prolonged accordingly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a steel for oil pipelines and a production method, specifically to an economical continuous oil pipe steel resistant to H2S corrosion and a production method thereof. Background Art

[0002] As a tool for oilfield operations, coiled tubing needs to withstand high pressure, fatigue, and even a corrosive environment containing H2S. For conventional coiled tubing, due to reasons of composition and process design, segregation of hard phase structures in the coiled tubing is likely to become a channel for hydrogen-induced cracking, resulting in the failure of the coiled tubing.

[0003] After retrieval:

[0004] The patent document with the Chinese patent application number 202010343865.3 discloses "A Quenched and Tempered Type Coiled Tubing Steel, Steel Strip and Preparation Method of Oil Casing". It contains the following chemical elements in mass percentages: C: 0.15 - 0.35%, Si: 0.08 - 0.30%, Mn: 0.50 - 1.80%, P ≤ 0.015%, S ≤ 0.005%, Cr: 0.40 - 0.80%, Nb: 0.01 - 0.05%, Ti: 0.01 - 0.03%, Mo: 0.05 - 0.38%, B: 0.0003 - 0.0015%, Ca: 0.001 - 0.004%, A1: 0.01 - 0.05%, 0 < N ≤ 0.006%; the steel pipe prepared has ultra-high strength, uniform tissue properties, and good fatigue life and corrosion resistance. Through the implementation of this patent, although an ultra-high strength quenched and tempered type coiled tubing can be obtained, from the perspectives of its structure and hardness and other characteristics, it does not have good H2S corrosion resistance.

[0005] The patent document with the Chinese patent application number 202210921398.7 discloses "A Stainless Steel Coiled Tubing and Its Preparation Method", which includes: butt-welding and lengthening a ferritic stainless steel strip, and successively performing cooling, tempering, and rolling treatments on the weld area; curling and forming the butt-welded and lengthened ferritic stainless steel strip; performing straight-weld welding on the curled and formed ferritic stainless steel strip; performing quenching treatment on the weld, and performing tempering treatment on the weld and the coiled tubing to obtain a stainless steel coiled tubing with a ferritic microstructure. Since the added Cr content is 13 - 15%, which is very high, although it has good H2S corrosion resistance, it is not economical. Summary of the Invention

[0006] The present invention aims to overcome the deficiencies of the existing technology, which is neither economical nor has poor H2S corrosion resistance, and provides an economical continuous oil pipe steel resistant to H2S corrosion and a production method thereof, which is relatively economical and can prevent the steel plate from cracking after quenching and tempering in terms of HIC and SSCC corrosion resistance.

[0007] Measures to achieve the above objectives:

[0008] An economical H2S corrosion resistant continuous oil pipe steel, the components and weight percentage of which are: C: 0.07-0.25%, Si: ≤0.48%, Mn: 0.33-1.28%, P: ≤0.016%, S: ≤0.0013%, Al: 0.014-0.041%, Nb: 0.008-0.057%, N: ≤0.0043%, O: ≤0.0023%, and Cu: ≤0.3 7%, Ni: ≤0.22%, Cr: ≤3.13%, Mo: ≤0.31%, V: ≤0.072%, Ti: ≤0.021%, B: ≤0.0005% any two or more, but not all of them are added at the same time; and Ca is controlled at 0.0010-0.0025% or Mg is controlled at 0.0006-0.0020%, or Ca and Mg are arbitrarily combined within their respective ranges, and the rest are iron and unavoidable impurities.

[0009] Preferably, among the following elements to be mixed and added, their weight percentage contents are: Cu: ≤0.32%, Ni: ≤0.19%, Cr: ≤2.93%, Mo: ≤0.28%, V: ≤0.067%, Ti: ≤0.019%, B: ≤0.00045%.

[0010] Preferably, the weight percentage of Ca is between 0.0013 and 0.0020%, or the weight percentage of Mg is between 0.0008 and 0.0016%.

[0011] A method for producing an economical H2S corrosion resistant coiled tubing steel, comprising the following steps:

[0012] 1) Continuous casting into batches after conventional smelting; during which, after the RH treatment, Ca treatment or Mg treatment or Ca-Mg composite treatment is performed, and the treatment amount is carried out according to the definition of claim 1;

[0013] 2) The ingot is heated, and the heating temperature of the ingot is controlled at 1150-1250°C, and T·(20+lg(t)) / 10000 is controlled at 2.30-2.55, where:

[0014] T—the highest temperature during the heating of the billet, in °C;

[0015] t—time from 1150℃ to the end of heating, in hours;

[0016] 3) Rolling is performed, and the final rolling temperature is controlled to be not less than 800°C;

[0017] 4) Cooling to the coiling temperature at a cooling rate of not less than 50°C / s;

[0018] 5) Coil the steel sheet and control the coiling temperature at 520-650°C.

[0019] Preferably, the final rolling temperature is controlled at 815-895°C.

[0020] Preferably, the coiling temperature is between 526 and 632°C.

[0021] Preferably, the cooling rate is between 55 and 95° C. / s.

[0022] The method comprises the following steps: after the RH treatment, a Ca treatment, a Mg treatment or a Ca-Mg composite treatment is carried out, and the treatment amount is carried out according to the limit specified in claim 1.

[0023] The functions and mechanisms of the components and main processes in the present invention are as follows:

[0024] Carbon (C): The most economical interstitial solid solution strengthening element, and also a strong hardenability element. It promotes martensite formation during quenching, and disperses and precipitates carbides during tempering to obtain a good match of strength and toughness. At the same time, the dispersed carbide particles can act as hydrogen traps to improve the material's resistance to H2S corrosion; but when the C content is too high, it is easy to cause serious component segregation, resulting in excessive local microhardness and becoming a source of hydrogen-induced cracking. The appropriate C content is 0.07-0.25%.

[0025] Silicon (Si): It mainly plays a role in solid solution strengthening and is beneficial to assist desulfurization during the smelting process. However, too high Si content can easily make it difficult to remove the surface oxide scale and cause uneven cooling during the cooling process, which in turn leads to uneven hardness of the material and deteriorates the material's resistance to hydrogen embrittlement. The appropriate Si content should be less than 0.48%.

[0026] Manganese (Mn): It can improve the hardenability of steel and significantly increase the yield and tensile strength of steel. However, Mn is an element that is easy to segregate. It will increase the stability of austenite in the segregated area, further aggravate the diffusion of C to the segregated area during the phase transformation, and finally form a brittle and hard martensite phase, which is not good for the toughness of the material; especially the severe segregation in the center of the plate thickness is often an important reason for fracture separation. The appropriate addition amount of Mn is 0.33-1.28%.

[0027] Chromium (Cr): It can improve the hardenability of steel, significantly increase the yield and tensile strength of steel, and promote the formation of a dense oxide film on the surface of steel, reducing the risk of hydrogen embrittlement. However, Cr is a precious alloy, and adding too much content can easily lead to an excessively high composition. The appropriate addition amount of Cr is ≤3.13%.

[0028] Molybdenum (Mo): It can improve the hardenability of steel and the stability of high temperature tempering performance, and can form Mo carbides, provide hydrogen traps, and improve the material's hydrogen resistance. Mo is also a precious alloy, and the appropriate addition amount is ≤0.31%.

[0029] Niobium and vanadium (Nb, V): They are easy to combine with C to form microalloy precipitates, and act as important hydrogen traps to improve the material's hydrogen resistance; at the same time, dispersed microalloy precipitates are also beneficial to improving the material's strength. The appropriate Nb content is 0.008-0.057%, and the V content is ≤0.072%.

[0030] Copper, nickel (Cu, Ni): Cu has a certain solid solution strengthening effect and improves the corrosion resistance of steel, but Cu should not be added alone; Ni can improve the low temperature toughness of the material and improve the surface brittleness caused by Cu. When it is necessary to improve the uniform corrosion resistance, Cu and Ni can be added appropriately, and the appropriate addition amount is Cu: ≤0.37%, Ni: ≤0.22%.

[0031] Calcium and magnesium (Ca, Mg): Ca and Mg can combine with S to avoid the formation of MnS and improve the acid resistance of the material; at the same time, Mg can make the inclusion distribution more dispersed, become solid hydrogen particles, and enhance the material's role in refining the weld and hot zone grains, thereby improving the toughness of the weld and hot zone.

[0032] The reason why the heating temperature of the ingot is controlled at 1150-1250°C is that when the temperature is too low, the alloy elements are not fully dissolved, which is not conducive to material segregation control, and when the temperature is too high, the coarse grains are not conducive to material toughness; at the same time, T·(20+lg(t)) / 10000 is controlled to be between 2.30 and 2.55 (where T is the maximum heating temperature (°C), and t is the heating time above 1150°C (h)), and good solid solution effect and grain size are obtained in this range.

[0033] The reason why the final rolling temperature is controlled to be not less than 800° C. in the present invention is to avoid two-phase rolling of the surface layer, which leads to uneven surface structure and ultimately uneven surface microscopic properties, thereby reducing the fatigue performance of the material.

[0034] The reason why the present invention controls the cooling to the coiling temperature at a cooling rate of not less than 50°C / s is that through rapid cooling, the diffusion of carbon is suppressed, and the carbon that has been homogenized in the austenite is prevented from re-diffusing back to the original area enriched with alloy elements such as Mn during cooling and phase transformation, resulting in the production of large pieces of pearlite, martensite islands and other hard phase structures. Through this measure, the pearlite and martensite islands are dispersed; during the quenching and heating process, the dispersed pearlite and martensite islands are conducive to the formation of an austenite grain structure with uniform organization and composition, ultimately improving the hydrogen resistance of the material.

[0035] The reason why the coiling temperature is controlled at 520-650°C in the present invention is that too high a temperature easily leads to the formation of pearlite bands or central martensite bands, which is detrimental to the final acid resistance; when the temperature is too low, the material strength and hardness are too high, which is detrimental to the pipe making performance.

[0036] Compared with the prior art, the present invention is relatively economical, and the steel plate has good HIC and SSCC corrosion resistance and will not crack after quenching and tempering, thereby improving the qualified rate of the prepared coiled tubing. In addition, compared with stainless steel, the alloy content of the coiled tubing product designed by the present invention greatly reduces the content of precious alloys such as Cr, thereby reducing the production cost. DETAILED DESCRIPTION

[0037] The present invention is described in detail below:

[0038] Table 1 is a list of chemical components of various embodiments and comparative examples of the present invention;

[0039] Table 2 is a list of main process parameters of various embodiments and comparative examples of the present invention;

[0040] Table 3 is a table of performance test results of various embodiments and comparative examples of the present invention.

[0041] Each embodiment of the present invention is produced according to the following steps

[0042] 1) Continuous casting into batches after conventional smelting; during which, after the RH treatment, Ca treatment or Mg treatment or Ca-Mg composite treatment is performed, and the treatment amount is carried out according to the definition of claim 1;

[0043] 2) The ingot is heated, and the heating temperature of the ingot is controlled at 1150-1250°C, and T·(20+lg(t)) / 10000 is controlled at 2.30-2.55, where:

[0044] T—the highest temperature during the heating of the billet, in °C;

[0045] t—time from 1150℃ to the end of heating, in hours;

[0046] 3) Rolling is performed, and the final rolling temperature is controlled to be not less than 800°C;

[0047] 4) Cooling to the coiling temperature at a cooling rate of not less than 50°C / s;

[0048] 5) Coil the steel sheet and control the coiling temperature at 520-650°C.

[0049] Table 1 Chemical composition list of various embodiments and comparative examples of the present invention (wt%)

[0050]

[0051]

[0052] Table 2 List of main process parameters of various embodiments of the present invention and comparative examples

[0053]

[0054] Table 3 List of mechanical properties test results of various embodiments of the present invention and comparative examples

[0055]

[0056]

[0057] Note: The HIC and SSC tests use NACE TM0284 A solution.

[0058] It can be seen from Table 3 that within the scope of the present invention, the material has good HIC and SSCC resistance, and the alloy content of the coiled tube product designed by the present invention is significantly reduced compared with that of stainless steel, and the content of precious alloys such as Cr is reduced, thereby reducing the production cost.

[0059] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.

Claims

1. An economical H2S corrosion resistant coiled tubing steel, the components and weight percentages of which are: C: 0.07-0.25%, Si: ≤0.48%, Mn: 0.33-1.28%, P: ≤0.016%, S: ≤0.0013%, Al: 0.014-0.041%, Nb: 0.008-0.057%, N: ≤0.0043%, O: ≤0.0023%, and Cu: ≤0.37%, Ni: ≤0.22%, Cr: Any two or more of ≤3.13%, Mo: ≤0.31%, V: ≤0.072%, Ti: ≤0.021%, B: ≤0.0005%, but not all of them are added at the same time; and Ca is controlled within 0.0010-0.0025% or Mg is controlled within 0.0006-0.0020%, or Ca and Mg are randomly combined within their respective ranges, and the rest are iron and unavoidable impurities.

2. The economical H2S corrosion resistant coiled tubing steel according to claim 1, characterized in that: The following elements to be mixed and added have a weight percentage content of: Cu: ≤0.32%, Ni: ≤0.19%, Cr: ≤2.93%, Mo: ≤0.28%, V: ≤0.067%, Ti: ≤0.019%, B: ≤0.00045%.

3. The economical H2S corrosion resistant coiled tubing steel according to claim 1, characterized in that: The weight percentage of Ca is 0.0013-0.0020% or the weight percentage of Mg is 0.0008-0.0016%.

4. A method for producing an economical H2S corrosion resistant coiled tubing steel as claimed in claim 1, comprising the following steps: 1) Continuous casting into batches after conventional smelting; during which, after the RH treatment, Ca treatment or Mg treatment or Ca-Mg composite treatment is performed, and the treatment amount is carried out according to the definition of claim 1; 2) The ingot is heated, and the heating temperature of the ingot is controlled at 1150-1250°C, and T·(20+lg(t)) / 10000 is controlled at 2.30-2.55, where: T—the highest temperature during the heating of the billet, in °C; t—time from 1150℃ to the end of heating, in hours; 3) Rolling is performed, and the final rolling temperature is controlled to be not less than 800°C; 4) Cooling to the coiling temperature at a cooling rate of not less than 50°C / s; 5) Coil the steel sheet and control the coiling temperature at 520-650°C.

5. The method for producing an economical H2S corrosion resistant coiled tubing steel according to claim 4, characterized in that: Control the final rolling temperature between 815 and 895°C.

6. The method for producing an economical H2S corrosion resistant coiled tubing steel according to claim 4, characterized in that: The coiling temperature is between 526 and 632°C.

7. The method for producing an economical H2S corrosion resistant coiled tubing steel according to claim 4, characterized in that: The cooling rate is between 55 and 95°C / s.

Citation Information

Patent Citations

  • Hot-rolled steel strip for CT90 level continuous pipe and production method of hot-rolled steel strip

    CN106498287A

  • Production of high tensile strength steel plate excellent in sour resistance and toughness at low temperature

    JP1994293919A

  • Method of manufacturing hot-rolled steel sheet and high strength steel pipe

    KR1020150050709A

Cited By

  • SA516Gr.70 steel plate resistant to hydrogen sulfide corrosion and production method of SA516Gr.70 steel plate

    CN121538558A