An in-situ generated Al4SiC4 reinforced aluminum-based composite material and a preparation method thereof
By using chopped silicon carbide fibers in aluminum-based composites, the problem of mismatch dislocation of ceramic particles and aluminum matrix is solved, the mechanical properties and thermal stability of the material are improved, and efficient Industrialized production.
Patent Information
- Application Number
- CN202411332727.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-24
AI Technical Summary
There is a mismatch dislocation in the interface between the ceramic particles and the aluminum matrix in the existing aluminum-based composite materials, resulting in insufficient mechanical properties and heat resistance of the material. The traditional preoxidation treatment method is complex and difficult to produce on a large scale.
Chopped silicon carbide fibers are used as the reaction raw material, and the Al4SiC4 reinforced phase is generated in situ through high-energy ball milling and strict control of sintering process parameters. Al elements react with the surface of silicon carbide fibers to eliminate free elements around the interface, and improve the mechanical properties and heat of the material. stability.
The mechanical properties of aluminum-based composite materials have been improved, the tensile strength reaches more than 879.67 MPa, and the process flow has been simplified, which facilitates large-scale industrial production and improves the thermal stability of the materials.
Smart Images

Figure CN118854192B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aluminum-based composite material, in particular to an in-situ generated Al4SiC4 reinforced aluminum-based composite material and a preparation method thereof, belonging to the technical field of reinforced phase modified composite materials. Background Art
[0002] With the development of modern industry, the performance of traditional materials can no longer meet the needs of high-end manufacturing. Aluminum-based composites have been widely used in aerospace, automobile manufacturing and other fields due to their excellent properties such as light weight, high strength, wear resistance and corrosion resistance. However, further improving the mechanical properties and heat resistance of aluminum-based composites is still an important research direction.
[0003] Particles are ideal obstacles to dislocation motion and are usually added to the metal matrix to increase the strength of the material. Ceramic particles (such as SiC, TiB2, and B4C) have also been introduced into these precipitation-hardened aluminum alloys to achieve ultra-high strength. However, misfit dislocations are prevalent at the interface between ceramic particles and the aluminum matrix, which attract alloying elements to nucleate at the interface, inducing coarse grain boundary phases and precipitation-free zones (PFZs) around the interface. These PFZ regions containing coarse phases are weak sites near the ceramic particle interface, where stress concentration usually occurs, thereby promoting early crack initiation. On the other hand, the formation of a large amount of coarse phases consumes alloying elements in the matrix, reduces the number density of fine precipitated phases, and weakens the precipitation strengthening of the composite. Therefore, the key issue of ceramic particle-reinforced metal matrix composites (MMCs) is to regulate the bonding between particles and the matrix.
[0004] The Chinese patent (CN114525434A) discloses a SiC-induced multiphase reinforced aluminum-based composite material and its preparation method. The SiC particles are pre-oxidized to form a SiO2 oxide layer, which improves the interface wettability between the SiC and the Al matrix and delays the reaction between the SiC particles and the Al matrix. At high temperatures, SiO2 will react with the matrix first, generating only a small amount of Al2O3 particles, and the SiC particles are basically retained. In the local area where the temperature is too high, a reaction will occur, which can completely consume the SiC particles there and generate Al2O3 particles. l4 SiC4 hard ceramic phase. However, the above method not only requires pre-oxidation of SiC particles, but also requires additive manufacturing. The tensile strength of the obtained material is only 400~450MPa, and it is difficult to mass-produce it industrially. Summary of the invention
[0005] In view of the problems existing in the prior art, the first purpose of the present invention is to provide an in-situ generated Al4SiC4 reinforced aluminum-based composite material. The composite material uses chopped silicon carbide fibers as reaction raw materials and utilizes Al element to react in situ on the surface of silicon carbide fibers to generate Al4SiC4 reinforcing phase. On the one hand, the dispersibility of silicon carbide fibers can be utilized to evenly disperse the Al4SiC4 reinforcing phase. On the other hand, free Si and C elements around the interface can be effectively eliminated, thereby purifying the grain boundaries, thereby further improving the thermal stability of the composite material.
[0006] The second object of the present invention is to provide a preparation method for in-situ generated Al4SiC4 reinforced aluminum-based composite materials. The method improves the surface activity of the raw materials through high-energy ball milling, and then strictly controls the sintering process parameters to control the Al matrix to be at the liquid-solid phase interface, thereby fully infiltrating the short-cut silicon carbide fibers and increasing the in-situ reaction contact area. The material is then strengthened by heat treatment, thereby greatly improving the mechanical properties of the material. The method is simple in process, easy to implement, and can be used for large-scale industrial production.
[0007] In order to achieve the above technical objectives, the present invention provides an in-situ generated Al4SiC4 reinforced aluminum-based composite material, comprising silicon carbide fiber and an in-situ generated Al4SiC4 reinforcement phase; the raw materials of the composite material include the following mass percentage components: Cu 2-5%, Mg 1-3%, Sn 0.1-1.5%, short-cut silicon carbide fiber 5-30%, and the balance Al;
[0008] The preparation process of the composite material is as follows: the raw materials are mixed evenly, mechanically activated, and then cold pressed to obtain a precursor; the precursor is subjected to programmed temperature sintering and then heat treated to obtain the composite material;
[0009] The mechanical activation method is high-energy ball milling, and the process is as follows: the raw materials are placed in a vacuum ball mill under a protective atmosphere and ground at a speed of 300-500 r / min for 5-12 h;
[0010] The process of programmed temperature sintering is as follows: in a protective atmosphere, the precursor is heated to 550-650° C. at a rate of 8-12° C. / min, kept at that temperature for 60-120 min, and then cooled to room temperature in the furnace.
[0011] As a preferred solution, the raw material also includes the following components in mass percentage: Fe≤0.1%, Mn≤0.1% and Sn≤0.1%.
[0012] As a preferred solution, the raw material consists of the following components in mass percentage: Cu 2-4%, Mg 1-2%, Sn 0.5-1%, short-cut silicon carbide fiber 5-15%, and the balance is Al.
[0013] As a preferred solution, the metal raw material in the raw material is a single substance powder, and its average particle size is -325 mesh.
[0014] As a preferred solution, the chopped silicon carbide fibers in the raw material have a diameter of 10-20 μm and a length of 80-120 μm.
[0015] As a preferred solution, the protective atmosphere is nitrogen and / or argon.
[0016] As a preferred solution, the ball-to-material ratio in the ball milling process is 1:0.1~2.
[0017] As a preferred solution, the cold pressing process is: placing the raw material after mechanical activation in a cold pressing mold, applying a pressure of 200~300MPa for cold pressing for 15~50s.
[0018] As a preferred solution, the process of programmed temperature sintering is: under a protective atmosphere, the precursor is heated to 600-620°C at 8-12°C / min, kept at this temperature for 100-120 minutes, and then cooled to room temperature in the furnace.
[0019] As a preferred solution, the heat treatment process includes quenching and artificial aging treatment.
[0020] As a preferred solution, after quenching, artificial aging treatment is performed at 160-180°C, and the aging treatment time is 10-20 hours.
[0021] The present invention controls the sintering temperature to be slightly lower than the melting point of aluminum, thereby ensuring that the Al element in the aluminum matrix partially reacts with the free C and Si elements in the short-cut silicon carbide fibers in a liquid-solid state, and Al4SiC4 is generated on the surface of the short-cut silicon carbide fibers, i.e., at the bonding interface between the aluminum matrix and the short-cut silicon carbide fibers. The chemical reaction is: 4Al + 3Si + 3C → Al4SiC4
[0022] Compared with the prior art, the beneficial technical effects of the present invention are:
[0023] 1) The aluminum-based composite material provided by the present invention uses short-cut silicon carbide fibers as reaction raw materials, and utilizes Al elements to react in situ on the surface of silicon carbide fibers to generate Al4SiC4 reinforcing phases. On the one hand, the dispersibility of silicon carbide fibers can be utilized to evenly disperse the Al4SiC4 reinforcing phases, and on the other hand, the free Si and C elements around the interface can be effectively eliminated, thereby playing a role in purifying the grain boundaries, thereby further improving the mechanical properties of the composite material.
[0024] 2) The preparation method provided by the present invention improves the surface activity of the raw materials through high-energy ball milling, and then strictly controls the sintering process parameters to control the sintering temperature to be slightly lower than the melting point of aluminum, thereby controlling the Al matrix to be at the liquid-solid phase interface, so as to fully infiltrate the chopped silicon carbide fibers, increase the contact area between the Al matrix and the silicon carbide fibers, and realize in-situ reaction without pretreatment of the raw materials. Then, the mechanical properties of the material are greatly improved by strengthening through heat treatment. The method is simple in process, easy to implement, and can be realized in large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the microstructure morphology of the prepared in-situ generated Al4SiC4 reinforced aluminum matrix composite material. DETAILED DESCRIPTION
[0026] Example 1
[0027] Step S1, powder preparation: Al powder, Cu powder, Mg powder, Sn powder, and short-cut silicon carbide fiber are prepared in a certain mass ratio: Cu: 4%, Mg: 2%, Sn: 1%, short-cut silicon carbide fiber: 10%, and the balance is Al;
[0028] Step S2, powder mixing: the ingredients in step S11 are placed in a vacuum ball mill with an inert atmosphere at a ball-to-material ratio of 1:1, and then the vacuum ball mill is placed on a ball mill for mixing at a speed of 300 r / min for 10 h, after which the mixed powder is taken out;
[0029] Step S3, cold pressing: the mixed powder in step S12 is cold pressed in Cr13 cold pressing die steel at a pressure of 200 MPa for 20 seconds;
[0030] Step S4, atmosphere sintering: the cold-pressed embryo in step S13 is placed in an atmosphere protection sintering furnace for sintering, the temperature is raised to 600°C at a heating rate of 10°C / min, and kept at this temperature for 120 minutes; then the sample is taken out after cooling to room temperature in the furnace;
[0031] Step S5, heat treatment: perform T6 heat treatment on the sample obtained in step S14, perform quenching treatment on the composite material at 520°C, and then perform artificial aging treatment at 170°C for 15 hours. The in-situ generated Al4SiC4 reinforced aluminum matrix composite material is obtained;
[0032] Step S6, processing the powder metallurgy precipitation strengthened cobalt-based high-temperature alloy obtained in step S15 into a powder metallurgy metal-based composite material standard tensile specimen, and performing a tensile test on a mechanical testing machine at a rate of 1 mm / min; the tensile strength is measured to be 879.67 MPa.
[0033] Example 2
[0034] This embodiment is exactly the same as Embodiment 1, except that:
[0035] Step S1: The raw material ratio is: Cu 2.5%, Mg 1.5%, Sn 0.3%, Fe 0.1%, Mn 0.1%, Cr 0.1%, short-cut silicon carbide fiber 5%, and the rest is Al;
[0036] Step S2: The ball-to-material ratio is 5:1, the ball milling time is 20 hours, the rotation speed is 500 r / min, and the tensile strength is measured to be 908.80 MPa.
[0037] Example 3
[0038] This embodiment is exactly the same as Embodiment 2, except that:
[0039] Step S1: The raw material ratio is: Cu 3.5%, Mg 1.5%, Sn 0.3%, Fe 0.1%, Mn 0.1%, Cr 0.1%, short-cut silicon carbide fiber 10%, and the rest is Al. The tensile strength is measured to be 806.15 MPa.
[0040] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations made to these embodiments without departing from the principles and spirit of the present invention are still within the protection scope of the present invention.
Claims
1. An in-situ generated Al4SiC4 reinforced aluminum matrix composite material, characterized by: The composite material comprises silicon carbide fibers and an Al4SiC4 reinforcement phase generated in situ; the raw materials of the composite material comprise the following components in mass percentage: Cu 2-5%, Mg 1-3%, Sn 0.1-1.5%, short-cut silicon carbide fibers 5-30%, and the balance Al; The preparation process of the composite material is as follows: the raw materials are mixed evenly, mechanically activated, and then cold pressed to obtain a precursor; the precursor is subjected to programmed temperature sintering and then heat treated to obtain the composite material; The mechanical activation method is high-energy ball milling, and the process is as follows: the raw materials are placed in a vacuum ball mill under a protective atmosphere and ground at a speed of 300-500 r / min for 5-12 h; The process of programmed temperature sintering is as follows: in a protective atmosphere, the precursor is heated to 550-650° C. at a rate of 8-12° C. / min, kept at that temperature for 60-120 min, and then cooled to room temperature in the furnace.
2. The in-situ generated Al4SiC4 reinforced aluminum-based composite material according to claim 1, characterized in that: The raw material also includes the following components in mass percentage: Fe≤0.1%, Mn≤0.1% and Sn≤0.1%.
3. The in-situ generated Al4SiC4 reinforced aluminum-based composite material according to claim 1, characterized in that: The raw material consists of the following components in mass percentage: Cu 2-4%, Mg 1-2%, Sn 0.5-1%, short-cut silicon carbide fiber 5-15%, and the balance is Al.
4. The method for preparing an in-situ generated Al4SiC4 reinforced aluminum-based composite material according to claim 1, characterized in that: The metal raw material in the raw material is a single substance powder with an average particle size of -325 mesh; the diameter of the short-cut silicon carbide fiber in the raw material is 10-20 μm and the length is 80-120 μm.
5. The method for preparing an in-situ generated Al4SiC4 reinforced aluminum-based composite material according to claim 1, characterized in that: The protective atmosphere is nitrogen and / or argon; the ball-to-material ratio in the ball milling process is 1:0.1-2.
6. The method for preparing an in-situ generated Al4SiC4 reinforced aluminum-based composite material according to claim 1, characterized in that: The cold pressing process is as follows: placing the mechanically activated raw material in a cold pressing mold, applying a pressure of 200-300 MPa for cold pressing for 15-50 seconds.
7. The method for preparing an in-situ generated Al4SiC4 reinforced aluminum-based composite material according to claim 1, characterized in that: The heat treatment process includes quenching and artificial aging treatment; after quenching, artificial aging treatment is performed at 160-180° C., and the aging treatment time is 10-20 hours.
Citation Information
Patent Citations
SiC-induced multi-phase reinforced aluminum-based composite material and preparation method thereof
CN114525434A
High-strength graphite fiber AlSiC composite material used for electronic packaging and preparation method thereof
CN106567021A
Preparation method of ultra-light and ultra-strong aluminum-based composite materials
CN112647028A
Silicon carbide fiber reinforced aluminum-based composite material as well as preparation method and application thereof
CN115679228A
Fiber reinforced metallic composite material
JP1982164946A