Composite shielding body for generating composite complex radiation environment for picosecond laser targeting
By using a multi-layer structure of precipitation-hardened stainless steel, transparent glass and porous carbon-loaded copper-cobalt bimetal shielding materials in a picosecond laser targeting environment, the problem of unsatisfactory pore distribution in porous carbon-based absorbing materials in the existing technology is solved, achieving It provides efficient shielding of picosecond laser composite radiation and is suitable for device protection and laser protection.
Patent Information
- Application Number
- CN202410906251.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Existing technology is difficult to effectively cope with the complex and complex radiation environment generated by picosecond laser targeting. The pore distribution of porous carbon-based absorbing materials is not ideal and cannot meet the needs for efficient electromagnetic pulse shielding.
Using a composite structure of a precipitation-hardened stainless steel layer, a transparent glass layer, a porous carbon-loaded copper-cobalt bimetallic shielding layer and a porous carbon-loaded copper metal shielding layer from the outside in, the porous carbon-loaded copper-cobalt bimetallic shielding layer is prepared through electrospinning and sintering processes. Metal and copper metal shielding materials form a multi-layer structure to synergistically shield electromagnetic radiation.
It achieves effective shielding of complex electromagnetic radiation generated by picosecond lasers. The composite shielding efficiency can reach more than 50%. It has good environmental adaptability and structural support and is suitable for device protection and laser protection.
Smart Images

Figure CN118870779A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite shielding body for generating a complex radiation environment for picosecond laser target shooting, belonging to the technical field of electromagnetic pulse shielding and protective materials. Background Art
[0002] With the rapid development of electronic technology, the functions and performance of electronic systems, weapon systems and other systems have also been greatly improved. At the same time, the impact of electromagnetic pulses in the above systems has also been strengthened. In many laser systems, the intensity of electromagnetic pulses generated by picosecond lasers is greater than that generated by nanosecond and femtosecond lasers, and the radiation environment generated by the interaction between picosecond lasers and solid targets is very complex, so there is an urgent need for an effective protection method for the complex radiation environment generated by picosecond laser target shooting. In addition, the distribution of pores in the existing research on porous carbon-based absorbing materials is still retained in the cross-section of the carbon material, such as the article "Porous carbon fiber absorbing composite materials and their influencing factors"; or it is impossible to use porous carbon materials to form a filamentous structure and use the holes on the silk or the pores formed between the silk to meet the quarter-wavelength absorption law as much as possible, such as the porous carbon absorbing material synthesized in the "Preparation of Boron Nitride Doped Porous Carbon Composite Materials and Research on Their Absorption Performance". Therefore, there is an urgent need for a process-controllable method for synthesizing porous carbon fibers. Summary of the invention
[0003] In view of this, an object of the present invention is to provide a composite shielding body for generating a complex radiation environment in picosecond laser targeting.
[0004] To achieve the above objectives, the technical solution of the present invention is as follows.
[0005] A composite shielding body for complex radiation environment generated by picosecond laser target shooting, comprising a precipitation hardened stainless steel layer, a first transparent glass layer, a porous carbon-loaded copper-cobalt bimetallic shielding layer, a second transparent glass layer, a porous carbon-loaded copper-metal shielding layer and a third transparent glass layer, which are arranged in sequence from the outside to the inside;
[0006] Wherein, the porous carbon-supported copper-cobalt bimetallic shielding layer is formed by mixing the porous carbon-supported copper-cobalt bimetallic shielding material with hot-melt paraffin and coating the mixture on the first transparent glass layer and the second transparent glass layer;
[0007] The porous carbon-loaded copper metal shielding layer is formed by mixing the porous carbon-loaded copper metal shielding layer material with hot-melt paraffin and coating the mixture on the second transparent glass layer and the third transparent glass layer.
[0008] Preferably, the thickness ratio of the precipitation hardened stainless steel layer, the first transparent glass layer, the porous carbon-loaded copper-cobalt bimetallic shielding layer, the second transparent glass layer, the porous carbon-loaded copper-metal shielding layer and the third transparent glass layer is 5 to 6: 1 to 2: 3 to 4: 1 to 2: 3 to 4: 1 to 2. More preferably, the thickness of the precipitation hardened stainless steel layer is 5 to 6 mm, the thickness of the first transparent glass layer, the second transparent glass layer and the third transparent glass layer are 1 to 2 mm respectively, and the thickness of the porous carbon-loaded copper-cobalt bimetallic shielding layer and the porous carbon-loaded copper-metal shielding layer are 3 to 4 mm respectively.
[0009] Preferably, the precipitation hardening stainless steel layer is made of 15-5PH precipitation hardening stainless steel.
[0010] Preferably, the volume ratio of the porous carbon-loaded copper-cobalt bimetallic shielding material to hot-melt paraffin is 5:5 to 6:4.
[0011] Preferably, the porous carbon-supported copper-cobalt bimetallic shielding material is prepared by the following method, which comprises the following steps:
[0012] (1) polyvinyl alcohol, copper nitrate trihydrate, cobalt nitrate hexahydrate and deionized water are mixed, heated to dissolve, polytetrafluoroethylene is added, and stirred to mix uniformly to obtain a spinning solution;
[0013] (2) electrospinning the spinning solution to obtain polymer fibers;
[0014] (3) placing the polymer fiber in a muffle furnace, heating the temperature to 280±10° C. at a heating rate of 2-3° C. / min, keeping the temperature for 2-3 hours, and cooling the temperature naturally to obtain pre-oxidized fiber;
[0015] (4) The pre-oxidized fiber is placed in a tubular furnace, and under a protective gas atmosphere, the temperature is first increased to 400-450°C at a heating rate of 2-3°C / min, then increased to 500-550°C at a heating rate of 0.8-1.2°C / min and kept warm for 1-2 h, and then increased to 700-800°C at a heating rate of 2-3°C / min and kept warm for 2-3 h, and naturally cooled to obtain a porous carbon-loaded copper-cobalt bimetallic shielding material.
[0016] Preferably, in step (1), the mass ratio of polyvinyl alcohol, copper nitrate trihydrate, cobalt nitrate hexahydrate and deionized water is 30-40:3-5:3-5:200; and the mass ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1.8-2.2.
[0017] Preferably, in step (2), during electrospinning, the temperature is 40-50°C, the humidity is 40%-50%, the positive voltage is 20-25KV, the negative voltage is -2-5KV, the flow rate is 0.05-1mm / min, and the receiving distance is 20-25cm.
[0018] Preferably, the volume ratio of the porous carbon-loaded copper metal shielding layer material to the hot-melt paraffin is 5:5 to 6:4.
[0019] Preferably, the porous carbon-supported copper metal shielding material is prepared by the following method, which comprises the following steps:
[0020] (1) polyvinyl alcohol, copper nitrate trihydrate and deionized water are mixed, heated to dissolve, polytetrafluoroethylene is added, and stirred to mix uniformly to obtain a spinning solution;
[0021] (2) electrospinning the spinning solution to obtain polymer fibers;
[0022] (3) placing the polymer fiber in a muffle furnace, heating the temperature to 280±10° C. at a heating rate of 2-3° C. / min, keeping the temperature for 2-3 hours, and cooling the temperature naturally to obtain pre-oxidized fiber;
[0023] (4) The pre-oxidized fiber is placed in a tubular furnace under a protective gas atmosphere, firstly heated to 400-450°C at a heating rate of 2-3°C / min, then heated to 500-550°C at a heating rate of 0.8-1.2°C / min and kept warm for 1-2 h, then heated to 700-800°C at a heating rate of 2-3°C / min and kept warm for 2-3 h, and then cooled naturally to obtain a porous carbon-loaded copper metal shielding material.
[0024] Preferably, in step (1), the mass ratio of polyvinyl alcohol, copper nitrate trihydrate and deionized water is 15-20:3-5:100; the mass ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1.8-2.2.
[0025] Preferably, in step (2), during electrospinning, the temperature is 40-50°C, the humidity is 40%-50%, the positive voltage is 20-25KV, the negative voltage is -2-5KV, the flow rate is 0.05-1mm / min, and the receiving distance is 20-25cm.
[0026] Beneficial Effects
[0027] The present invention provides a composite shielding body for complex radiation environment generated by picosecond laser target shooting. Precipitation hardened stainless steel, transparent glass, porous carbon-loaded copper-cobalt bimetal shielding material and porous carbon-loaded copper-metal shielding material are composited in a specific layer structure, and the layers work together to achieve shielding protection for complex electromagnetic radiation generated by picosecond laser and solid target, including effective shielding and absorption of charged particles such as electrons, photons such as gamma rays and other particles. The composite shielding body has strong environmental adaptability and can effectively shield electromagnetic pulses generated by the target chamber of a large picosecond kilojoule laser device. The composite shielding effectiveness can reach more than 50%, and can be applied to various fields such as device protection and laser protection.
[0028] The present invention provides a composite shielding body for the complex radiation environment generated by picosecond laser target shooting. The precipitation hardened stainless steel layer has high strength and corrosion resistance, can withstand the physical and chemical impact of the external environment, and protect the internal shielding layer from damage; secondly, the high atomic number atoms contained therein can effectively absorb photons, and effectively reduce the impact of charged particles through grounding, forming a preliminary electromagnetic isolation, and reducing the direct impact of the external electromagnetic field on the inner layer material. The transparent glass layer has good transparency to ensure that the light transmission is not affected. Secondly, it can be used as a carrier of the porous carbon-loaded metal shielding layer, so that the shielding material is well fixed in the corresponding position, providing structural support for the entire shielding system; finally, the transparent glass itself does not have an electromagnetic shielding function, but as a non-conductive material, it can reduce the reflection of electromagnetic waves and avoid the formation of unnecessary standing waves or reflected waves inside the shielding system. The porous carbon material in the porous carbon-loaded copper-cobalt bimetallic shielding material can effectively absorb and scatter electromagnetic waves due to its excellent conductivity and porous structure; metal copper has good electrical conductivity, which can effectively improve the imaginary part of the dielectric constant loss; metal cobalt, as a magnetic metal, can effectively improve the magnetic permeability of the material, thereby improving the material's magnetic loss capacity; through the interaction between metals, the impedance matching performance of the material can be effectively improved, allowing electromagnetic waves to interact with the material with less reflection. The porous carbon-loaded copper-cobalt bimetallic shielding layer and the transparent glass layer form an effective electromagnetic shielding, which can reduce the electromagnetic waves from continuing to penetrate the inner layer, and at the same time work together with the outer precipitation hardened stainless steel layer to form a double electromagnetic barrier to improve the overall shielding effect. The porous carbon-loaded copper metal shielding layer has good conductivity and cooperates with the outer structure to reduce the impact of electromagnetic waves on the inside of the shielding system.
[0029] The present invention provides a composite shielding body for the complex radiation environment generated by picosecond laser targeting. The porous carbon-loaded copper-cobalt bimetallic shielding material and the porous carbon-loaded copper-metal shielding material are prepared by spinning, pre-oxidation and sintering. They have excellent physical and chemical properties, simple preparation process, low raw material price, good stability and good shielding performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a modeling diagram of the composite shielding body of the present invention.
[0031] Figure 2 It is a schematic diagram of the structure of the composite shielding body of the present invention.
[0032] Figure 3 This is the X-ray diffraction pattern of the porous carbon-loaded copper metal shielding material in Example 1 of the present invention.
[0033] Figure 4 This is a microscopic morphology of the porous carbon-loaded copper metal shielding material in Example 1 of the present invention.
[0034] Figure 5 This is a microscopic morphology of the porous carbon-loaded copper metal shielding material in Comparative Example 1 of the present invention.
[0035] Figure 6 This is the X-ray diffraction pattern of the porous carbon-loaded copper-cobalt bimetallic shielding material in Example 2 of the present invention.
[0036] Figure 7 This is a microscopic morphology of the porous carbon-loaded copper-cobalt bimetallic shielding material in Example 2 of the present invention.
[0037] Figure 8 This is a microscopic morphology of the porous carbon-loaded copper-cobalt bimetallic shielding material in Comparative Example 2 of the present invention.
[0038] Fig. 9 This is a time domain diagram of the electromagnetic pulse signal in the target chamber of the kilojoule-class laser device in Example 3 of the present invention.
[0039] Fig.10 It is the amplitude of the electromagnetic pulse signal inside and outside the 15-5ph precipitation hardened stainless steel shielding box in the target chamber of the kilojoule-class laser device in Example 3 of the present invention.
[0040] Fig.11 The amplitude of electromagnetic pulse signals inside and outside the 15-5 ph precipitation hardened stainless steel shielding box was measured multiple times in the target chamber of the kilojoule-class laser device in Example 3 of the present invention.
[0041] Fig.12 The distribution relationship of the complex dielectric constant ε and the complex magnetic permeability μ of the porous carbon-loaded copper metal shielding material in Example 3 of the present invention in the 0.1-8 GHz band.
[0042] Fig.13 The distribution relationship of the complex dielectric constant ε and complex magnetic permeability μ of the porous carbon-loaded copper-cobalt bimetallic shielding material in the range of 0.1-8 GHz in Example 3 of the present invention. DETAILED DESCRIPTION
[0043] The present invention will be further described in detail below in conjunction with specific embodiments.
[0044] like Figure 1-2 As shown, a composite shielding body for generating a complex radiation environment for picosecond laser target shooting comprises a precipitation hardened stainless steel layer, a first transparent glass layer, a porous carbon-loaded copper-cobalt bimetallic shielding layer, a second transparent glass layer, a porous carbon-loaded copper-metal shielding layer and a third transparent glass layer, which are sequentially arranged from the outside to the inside;
[0045] Wherein, the porous carbon-supported copper-cobalt bimetallic shielding layer is formed by mixing the porous carbon-supported copper-cobalt bimetallic shielding material with hot-melt paraffin and coating the mixture on the first transparent glass layer and the second transparent glass layer;
[0046] The porous carbon-loaded copper metal shielding layer is formed by mixing the porous carbon-loaded copper metal shielding layer material with hot-melt paraffin and coating the mixture on the second transparent glass layer and the third transparent glass layer.
[0047] In some embodiments, the thickness ratio of the precipitation hardened stainless steel layer, the first transparent glass layer, the porous carbon-loaded copper-cobalt bimetallic shielding layer, the second transparent glass layer, the porous carbon-loaded copper metal shielding layer and the third transparent glass layer is 5-6:1-2:3-4:1-2:3-4:1-2.
[0048] In some embodiments, the thickness of the precipitation hardened stainless steel layer is 5 to 6 mm, the thickness of the first transparent glass layer, the second transparent glass layer and the third transparent glass layer are 1 to 2 mm respectively, and the thickness of the porous carbon-loaded copper-cobalt bimetallic shielding layer and the porous carbon-loaded copper metal shielding layer are 3 to 4 mm respectively.
[0049] In some embodiments, the precipitation hardened stainless steel layer is made of 15-5PH precipitation hardened stainless steel.
[0050] In some embodiments, the volume ratio of the porous carbon-supported copper-cobalt bimetallic shielding material to hot-melt paraffin is 5:5 to 6:4.
[0051] In some embodiments, the porous carbon-supported copper-cobalt bimetallic shielding material is prepared by the following method, which comprises:
[0052] (1) polyvinyl alcohol, copper nitrate trihydrate, cobalt nitrate hexahydrate and deionized water are mixed, heated to dissolve, polytetrafluoroethylene is added, and stirred to mix uniformly to obtain a spinning solution;
[0053] (2) electrospinning the spinning solution to obtain polymer fibers;
[0054] (3) placing the polymer fiber in a muffle furnace, heating the temperature to 280±10° C. at a heating rate of 2-3° C. / min, keeping the temperature for 2-3 hours, and cooling the temperature naturally to obtain pre-oxidized fiber;
[0055] (4) The pre-oxidized fiber is placed in a tubular furnace, and under a protective gas atmosphere, the temperature is first increased to 400-450°C at a heating rate of 2-3°C / min, then increased to 500-550°C at a heating rate of 0.8-1.2°C / min and kept warm for 1-2 h, and then increased to 700-800°C at a heating rate of 2-3°C / min and kept warm for 2-3 h, and naturally cooled to obtain a porous carbon-loaded copper-cobalt bimetallic shielding material.
[0056] In some embodiments, in step (1), the mass ratio of polyvinyl alcohol, copper nitrate trihydrate, cobalt nitrate hexahydrate and deionized water is 30-40:3-5:3-5:200; the mass ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1.8-2.2.
[0057] In some embodiments, in step (2), during electrospinning, the temperature is 40-50°C, the humidity is 40%-50%, the positive voltage is 20-25KV, the negative voltage is -2-5KV, the flow rate is 0.05-1mm / min, and the receiving distance is 20-25cm.
[0058] In some embodiments, the volume ratio of the porous carbon-supported copper metal shielding layer material to the hot melt paraffin is 5:5 to 6:4.
[0059] In some embodiments, the porous carbon-supported copper metal shielding material is prepared by the following method, the method steps comprising:
[0060] (1) polyvinyl alcohol, copper nitrate trihydrate and deionized water are mixed, heated to dissolve, polytetrafluoroethylene is added, and stirred to mix uniformly to obtain a spinning solution;
[0061] (2) electrospinning the spinning solution to obtain polymer fibers;
[0062] (3) placing the polymer fiber in a muffle furnace, heating the temperature to 280±10° C. at a heating rate of 2-3° C. / min, keeping the temperature for 2-3 hours, and cooling the temperature naturally to obtain pre-oxidized fiber;
[0063] (4) The pre-oxidized fiber is placed in a tubular furnace under a protective gas atmosphere, firstly heated to 400-450°C at a heating rate of 2-3°C / min, then heated to 500-550°C at a heating rate of 0.8-1.2°C / min and kept warm for 1-2 h, then heated to 700-800°C at a heating rate of 2-3°C / min and kept warm for 2-3 h, and then cooled naturally to obtain a porous carbon-loaded copper metal shielding material.
[0064] In some embodiments, in step (1), the mass ratio of polyvinyl alcohol, copper nitrate trihydrate and deionized water is 15-20:3-5:100; the mass ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1.8-2.2.
[0065] In some embodiments, in step (2), during electrospinning, the temperature is 40-50°C, the humidity is 40%-50%, the positive voltage is 20-25KV, the negative voltage is -2-5KV, the flow rate is 0.05-1mm / min, and the receiving distance is 20-25cm.
[0066] Example 1
[0067] In this embodiment, copper nitrate trihydrate has an analytical purity of 99.9% and a molecular weight of 241.6, and is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; the carbon source is an organic compound polyvinyl alcohol (PVA), which is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; and the pore-forming agent is an organic compound polytetrafluoroethylene dispersion (PTFE), which is purchased from Shanghai Myrel Chemical Technology Co., Ltd.
[0068] 1.5g PVA was mixed with 0.3g copper nitrate trihydrate and added to 10mL deionized water, heated in a water bath at 90°C, 500r / min for 180 minutes, and after stirring was completed and cooled to room temperature, 3g PTFE was added, and the mixed solution was stirred at room temperature for 12 hours to prepare a spinning solution. Subsequently, a SS-2535H electrospinning machine purchased by Beijing Yongkang Leye Technology Development Co., Ltd. was used to construct a filamentous structure, and the spinning solution was loaded into a 10ml syringe to ensure that the spinning solution ejection point was 22cm away from the receiving roller, and a positive voltage of 22kV and a negative voltage of -2kV were applied. Electrospinning was performed at a push speed of 0.06mm / min at 40% humidity and a constant temperature of 40°C to obtain a polymer spinning fiber. The polymer spinning fiber was pre-oxidized in a KSL-1200X muffle furnace purchased by Hefei Kejing Material Technology Co., Ltd., with a heating rate of 2°C / min and a termination temperature of 280°C. After two hours of heat preservation, the temperature was naturally lowered. After cooling down, the above materials were placed in an OTF-1200X tubular furnace purchased by Hefei Kejing Material Technology Co., Ltd. for ventilation sintering. The gas introduced was argon. Starting from room temperature, the temperature was raised to 400°C at a heating rate of 2°C / min, then raised to 500°C at a heating rate of 1°C / min, and then kept at 500°C for 1 hour, and then raised to 800°C at a heating rate of 2°C / min. After keeping for two hours, the temperature was naturally lowered. After cooling, the porous carbon-supported single metal copper shielding material was taken out to obtain.
[0069] The X-ray diffraction results of the porous carbon-supported single-metal copper shielding material are as follows: Figure 3 The scanning electron microscopy results are shown in Figure 4 shown.
[0070] Comparative Example 1
[0071] In this comparative example, during sintering, the temperature was directly raised to 800°C at a heating rate of 2°C / min, kept at that temperature for two hours, and then naturally cooled. The rest was the same as in Example 1, to obtain a porous carbon-loaded single-metal copper shielding material.
[0072] The scanning electron microscopy results of the porous carbon-supported single-metal copper shielding material are as follows: Figure 5 shown.
[0073] Example 2
[0074] In this embodiment, copper nitrate trihydrate has an analytical purity of 99.9% and a molecular weight of 241.6, which is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; cobalt nitrate hexahydrate has an analytical purity of 99% and a molecular weight of 291.03, which is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; the carbon source is an organic compound polyvinyl alcohol (PVA), which is purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; the pore-forming agent is an organic compound polytetrafluoroethylene dispersion (PTFE), which is purchased from Shanghai Myrel Chemical Technology Co., Ltd.
[0075] 1.5g PVA was mixed with 0.15g copper nitrate trihydrate and 0.15g cobalt nitrate hexahydrate, and then added to 10mL deionized water, and heated in a water bath at 90°C and 500r / min for 180 minutes. After stirring and cooling to room temperature, 3g PTFE was added, and the mixed solution was stirred at room temperature for 12 hours to prepare a spinning solution. Subsequently, a SS-2535H electrospinning machine purchased by Beijing Yongkang Leye Technology Development Co., Ltd. was used to construct a filamentous structure, and the spinning solution was loaded into a 10ml syringe, ensuring that the spinning solution ejection point was 22cm away from the receiving drum, applying a positive voltage of 22kV and a negative voltage of -2kV, and electrospinning was performed at a push speed of 0.06mm / min at 40% humidity and a constant temperature of 40°C to obtain polymer spinning fibers. The polymer spinning fiber is pre-oxidized in a KSL-1200X muffle furnace purchased by Hefei Kejing Material Technology Co., Ltd., with a heating rate of 2°C / min and a termination temperature of 280°C. After two hours of heat preservation, the material is placed in an OTF-1200X tubular furnace purchased by Hefei Kejing Material Technology Co., Ltd. for ventilation sintering. The gas introduced is argon. Starting from room temperature, the temperature is increased to 400°C at a heating rate of 2°C / min, and then increased to 500°C at a heating rate of 1°C / min, and then kept at 500°C for 1 hour, and then increased to 800°C at a heating rate of 2°C / min. After two hours of heat preservation, the temperature is naturally cooled. After cooling, the porous carbon-loaded copper-cobalt bimetallic shielding material is obtained.
[0076] The X-ray diffraction results of the porous carbon-supported copper-cobalt bimetallic shielding material are as follows: Figure 6The scanning electron microscopy results are shown in Figure 7 shown.
[0077] Comparative Example 2
[0078] In this comparative example, during sintering, the temperature was directly raised to 800° C. at a heating rate of 2° C. / min, kept at that temperature for two hours, and then naturally cooled. The rest was the same as in Example 1, to obtain a porous carbon-supported copper-cobalt bimetallic shielding material.
[0079] The scanning electron microscopy results of the porous carbon-supported copper-cobalt bimetallic shielding material are as follows: Figure 8 shown.
[0080] contrast Figure 4-5 , Figure 7-8 From the results, it can be seen that in the process of preparing porous carbon-loaded single-metal copper shielding materials and porous carbon-loaded copper-cobalt bimetallic shielding materials, regulating the heating method is one of the key steps to optimize the microstructure and performance of the material. In Comparative Example 1, before the heating curve was adjusted, the observed material morphology showed obvious deficiencies. Specifically, the size of the metal particles appears to be abnormally large, which not only increases the surface roughness of the material, but also has an adverse effect on the overall properties of the material such as conductivity and mechanical strength. At the same time, the embedding method of these large-sized metal particles in the filamentous carbon structure is also not ideal, resulting in significant connection between the holes in the filamentous structure. This excessive connection not only weakens the integrity and stability of the filamentous structure, but may also affect the key properties of the material such as permeability, thereby destroying its original design intention and functional advantages to a certain extent.
[0081] In Example 1, by introducing a gentler heating rate, setting a suitable temperature platform and precise temperature control, precise control of phase change and crystal growth behavior during material synthesis is achieved. This improvement has brought about significant changes: the size of the metal particles has been significantly refined, their distribution has become more uniform, and they are more closely embedded in the filamentous carbon structure, reducing the proportion exposed to the outside, which not only enhances the interaction between the metal and the carbon matrix, but also promotes electron transmission and energy exchange between the two, bringing better overall performance to the material.
[0082] In addition, the optimized heating method also led to positive changes in the pore distribution on the filamentous carbon structure. The number and size of the pores were reasonably regulated, which not only retained sufficient pore space to maintain the high specific surface area and good permeability of the material, but also avoided excessive adhesion between the pores, ensuring the uniformity and independence of the pore distribution. This optimization of the pore structure can improve the mechanical properties and thermal stability of the material to a certain extent.
[0083] In summary, through scientific regulation of the heating method, not only the problems of excessive metal particle size and connected pores were successfully solved, but also a closer bond between the filamentous carbon structure and the metal and the optimization of the pore structure were achieved.
[0084] Example 3
[0085] A composite shielding body for complex radiation environment generated by picosecond laser target shooting, comprising a precipitation hardened stainless steel layer, a first transparent glass layer, a porous carbon-loaded copper-cobalt bimetallic shielding layer, a second transparent glass layer, a porous carbon-loaded copper-metal shielding layer and a third transparent glass layer, which are arranged in sequence from the outside to the inside;
[0086] The porous carbon-supported copper-cobalt bimetallic shielding layer is formed by mixing the porous carbon-supported copper-cobalt bimetallic shielding material prepared in Example 2 with hot-melt wax and then coating the mixture on the first transparent glass layer and the second transparent glass layer; the volume ratio of the porous carbon-supported copper-cobalt bimetallic shielding material to the hot-melt wax is 6:4;
[0087] The porous carbon-loaded copper metal shielding layer is formed by mixing the porous carbon-loaded copper metal shielding layer material prepared in Example 1 with hot-melt wax and then coating it on the second transparent glass layer and the third transparent glass layer; the volume ratio of the porous carbon-loaded copper metal shielding layer material to the hot-melt wax is 6:4.
[0088] The thickness of the precipitation hardened stainless steel layer is 5 mm, the thickness of the first transparent glass layer, the second transparent glass layer and the third transparent glass layer are 1 mm respectively, and the thickness of the porous carbon-loaded copper-cobalt bimetallic shielding layer and the porous carbon-loaded copper metal shielding layer are 3 mm respectively.
[0089] The material of the precipitation hardening stainless steel layer is 15-5PH precipitation hardening stainless steel.
[0090] The precipitation hardened stainless steel, porous carbon loaded copper-cobalt bimetallic shielding material, and porous carbon loaded copper metal shielding layer material were tested respectively:
[0091] A 15-5ph precipitation hardened stainless steel shielding box is placed in the picosecond laser target chamber, and signal receiving antennas are connected inside and outside the shielding box for comparison. The antennas inside and outside the shielding box are placed in the same position in the target chamber for comparison. After the electromagnetic pulse is generated, the magnetic field antenna can be connected to an oscilloscope of appropriate range through a cable and attenuator for collection. Fig. 9The laser parameters for obtaining electromagnetic pulses are ps-60.6J, 812fs; the solid target interacting with the picosecond laser is a 20μm CH wire target. An antenna is placed in a shielding box 80cm behind the target, and a bare open antenna without shielding box protection is placed at the same distance. After the picosecond laser interacts with the solid target to generate an electromagnetic pulse signal, it is shielded by a 15-5ph precipitation hardened stainless steel shielding box. The results are as follows Fig.10 As shown, the electromagnetic pulse intensity of the bare antenna detection is 1173kV / m, while the electromagnetic pulse amplitude of the antenna detected in the 15-5ph precipitation-hardened stainless steel shielding box is 431kV / m. The electromagnetic pulse signal intensity is reduced by more than half, the attenuation efficiency is about 63.6%, and the shielding effect is more significant.
[0092] In order to avoid accidental errors in the experiment, multiple experimental tests and comparisons were conducted in this application, and multiple experiments were conducted using a kilojoule-level laser device. The results are as follows Fig.11 As shown, in the three experiments, the detection results of the antenna in the shielding box all showed obvious attenuation, and the attenuation efficiency was above 50% compared with the antenna without the shielding box.
[0093] In order to test the electromagnetic pulse shielding performance of porous carbon-loaded single-metal copper shielding material and porous carbon-loaded copper-cobalt bimetal shielding material, the above two materials were mixed with hot-melt paraffin in a volume ratio of 6:4 and melted and then pressed into rings. Fig.12 The distribution of complex dielectric constant and complex magnetic permeability in the frequency range of 0.1-8GHz after the porous carbon-loaded single-metal copper shielding material is pressed into a hollow cylindrical shielding body with an inner diameter of 3mm, an outer diameter of 7mm, and a height of 3.15mm. The dielectric loss and magnetic loss of the shielding material can be measured by the ratio of the imaginary part to the real part of the complex dielectric constant and the ratio of the imaginary part to the real part of the complex magnetic permeability. Fig.12 The measured data shows that the dielectric loss of this material is better than the magnetic loss and the difference is large, so the impedance matching needs to be adjusted, and therefore a variety of materials are used for progressive shielding.
[0094] like Fig.13 As shown, within the test frequency band, the porous carbon-loaded copper-cobalt bimetallic shielding material and hot-melt paraffin were mixed and melted in a volume ratio of 6:4 and pressed into a hollow cylindrical shielding body with an inner diameter of 3mm, an outer diameter of 7mm, and a height of 2.72mm for testing. Since the magnetic metal element cobalt is added to the absorbing material, the magnetic loss capacity of the porous carbon-loaded copper-cobalt bimetallic shielding material is greatly improved, and the dielectric loss does not change much, so the porous carbon-loaded copper-cobalt bimetallic shielding material has better impedance matching.
[0095] In the shielding system described in this embodiment, the selection and arrangement of the materials of each layer are intended to provide multiple barriers to minimize the penetration and interference of electromagnetic waves. The following is a detailed analysis of the role and coupling relationship between the layers:
[0096] Outer layer: 15-5PH precipitation hardened stainless steel shielding box: 15-5PH alloy is an ideal material for the outer shielding box due to its high strength (tensile strength can reach more than 1700MPa, yield strength can reach more than 1400MPa), high corrosion resistance (especially in high temperature and humid environment) and good processing performance. It can withstand the physical and chemical impact of the external environment and protect the internal shielding layer from damage. Secondly, it contains high atomic number atoms that can effectively absorb photons, and effectively reduce the impact of charged particles through grounding, forming a preliminary electromagnetic isolation, reducing the direct impact of external electromagnetic fields on the inner layer material.
[0097] The second layer: transparent glass, its good transparency can ensure that light transmission is not affected; secondly, as an intermediate layer, it provides structural support for the entire shielding system and can be used as a carrier of shielding materials to better fix the shielding materials in the corresponding positions; finally, transparent glass itself does not have electromagnetic shielding function, but as a non-conductive material, it can reduce the reflection of electromagnetic waves and avoid the formation of unnecessary standing waves or reflected waves inside the shielding system.
[0098] The third layer: a 3 mm thick shielding material prepared by mixing porous carbon-loaded copper-cobalt bimetallic shielding material and hot-melt paraffin. The porous carbon material can effectively absorb and scatter electromagnetic waves due to its excellent conductivity and porous structure. The addition of copper and cobalt bimetallics further enhances its conductivity and electromagnetic shielding performance, and effectively regulates the relationship between the complex dielectric constant and the complex magnetic permeability, thereby improving the impedance matching, which can make the electromagnetic waves interact with the shielding material with less reflection, and greatly reduce the impact of the electromagnetic field on the inside in this layer. At the same time, hot-melt paraffin is used as a matrix material. By adjusting the ratio of its use with the porous carbon-loaded copper-cobalt bimetallic shielding material, the absorption and reflection capacity of the shielding material can be effectively adjusted. An effective electromagnetic shielding layer is formed between the inner transparent glass layer, reducing the possibility of electromagnetic waves continuing to penetrate the inner layer. And it works together with the outer stainless steel shielding box to form a double electromagnetic barrier to improve the overall shielding effect.
[0099] The fourth layer: transparent glass. This layer has the same function as the second layer, connecting the inner and outer layers of shielding materials to ensure the integrity and stability of the overall structure.
[0100] The fifth layer: a 3mm thick shielding material made of porous carbon-loaded copper single metal shielding material and hot melt paraffin, similar to the third layer, but with a single metal copper load, the material only has good conductivity. Although it cannot completely reduce the electromagnetic wave reflection like the third layer, the reflected electromagnetic wave will still act on the previous layers of materials. Therefore, this layer is to minimize the impact of electromagnetic waves on the inside of the shielding system.
[0101] The sixth layer: transparent glass. The function of this layer is the same as the above two layers of transparent glass, that is, it plays a fixed supporting role and forms the final electromagnetic shielding layer with the fifth layer to ensure that the internal equipment or space is protected from external electromagnetic interference.
[0102] In summary, the present invention provides a shielding method for the complex radiation environment generated by picosecond laser target shooting, using 15-5ph precipitation hardened stainless steel as the outer shell of the absorption system to protect the internal porous carbon-loaded single metal copper shielding material and the porous carbon-loaded copper and cobalt bimetallic shielding material, so that the method has stronger environmental adaptability, and can effectively shield the electromagnetic pulses generated by the target chamber of the picosecond kilojoule-class large laser device, the composite shielding effectiveness can reach more than 50%, and can be applied to various fields such as device protection and laser protection. It can be further used in conjunction with a grounding system or an electromagnetic interference suppressor to improve the overall electromagnetic shielding effect and anti-interference ability.
[0103] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A composite shield for complex radiation environment generated by picosecond laser targeting. Features: It includes a precipitation hardened stainless steel layer, a first transparent glass layer, a porous carbon-loaded copper-cobalt bimetallic shielding layer, a second transparent glass layer, a porous carbon-loaded copper-metal shielding layer and a third transparent glass layer, which are arranged in sequence from the outside to the inside; Wherein, the porous carbon-supported copper-cobalt bimetallic shielding layer is formed by mixing the porous carbon-supported copper-cobalt bimetallic shielding material with hot-melt paraffin and coating the mixture on the first transparent glass layer and the second transparent glass layer; The porous carbon-loaded copper metal shielding layer is formed by mixing the porous carbon-loaded copper metal shielding layer material with hot-melt paraffin and coating the mixture on the second transparent glass layer and the third transparent glass layer.
2. A composite shielding body for generating a complex radiation environment for picosecond laser targeting as claimed in claim 1, Features: The thickness ratio of the precipitation hardened stainless steel layer, the first transparent glass layer, the porous carbon-loaded copper-cobalt bimetallic shielding layer, the second transparent glass layer, the porous carbon-loaded copper-metal shielding layer and the third transparent glass layer is 5-6:1-2:3-4:1-2:3-4:1-2.
3. A composite shielding body for generating a complex radiation environment for picosecond laser target shooting as claimed in claim 2, Features: The thickness of the precipitation hardened stainless steel layer is 5-6 mm, the thickness of the first transparent glass layer, the second transparent glass layer and the third transparent glass layer are 1-2 mm respectively, and the thickness of the porous carbon-loaded copper-cobalt bimetallic shielding layer and the porous carbon-loaded copper metal shielding layer are 3-4 mm respectively.
4. A composite shielding body for generating a complex radiation environment for picosecond laser targeting as claimed in claim 1, Features: The material of the precipitation hardening stainless steel layer is 15-5PH precipitation hardening stainless steel.
5. A composite shielding body for generating a complex radiation environment for picosecond laser targeting as claimed in claim 1, Features: The volume ratio of the porous carbon-loaded copper-cobalt bimetallic shielding material to the hot-melt paraffin is 5:5 to 6:
4.
6. A composite shielding body for generating a complex radiation environment for picosecond laser targeting as claimed in claim 1, Features: The porous carbon-supported copper-cobalt bimetallic shielding material is prepared by the following method, which comprises the following steps: (1) polyvinyl alcohol, copper nitrate trihydrate, cobalt nitrate hexahydrate and deionized water are mixed, heated to dissolve, polytetrafluoroethylene is added, and stirred to mix uniformly to obtain a spinning solution; (2) electrospinning the spinning solution to obtain polymer fibers; (3) placing the polymer fiber in a muffle furnace, heating the temperature to 280±10° C. at a heating rate of 2-3° C. / min, keeping the temperature for 2-3 hours, and cooling the temperature naturally to obtain pre-oxidized fiber; (4) The pre-oxidized fiber is placed in a tubular furnace, and under a protective gas atmosphere, the temperature is first increased to 400-450°C at a heating rate of 2-3°C / min, then increased to 500-550°C at a heating rate of 0.8-1.2°C / min and kept warm for 1-2 h, and then increased to 700-800°C at a heating rate of 2-3°C / min and kept warm for 2-3 h, and naturally cooled to obtain a porous carbon-loaded copper-cobalt bimetallic shielding material.
7. A composite shielding body for generating a complex radiation environment for picosecond laser target shooting as claimed in claim 6, Features: In step (1), the mass ratio of polyvinyl alcohol, copper nitrate trihydrate, cobalt nitrate hexahydrate and deionized water is 30-40:3-5:3-5:200; the mass ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1.8-2.2; In step (2), during electrospinning, the temperature is 40-50° C., the humidity is 40%-50%, the positive voltage is 20-25 KV, the negative voltage is -2-5 KV, the flow rate is 0.05-1 mm / min, and the receiving distance is 20-25 cm.
8. A composite shielding body for generating a complex radiation environment for picosecond laser target shooting as claimed in claim 1, Features: The volume ratio of the porous carbon-loaded copper metal shielding layer material to the hot-melt paraffin is 5:5 to 6:
4.
9. A composite shielding body for generating a complex radiation environment for picosecond laser targeting as claimed in claim 1, Features: The porous carbon-loaded copper metal shielding material is prepared by the following method, which comprises the following steps: (1) polyvinyl alcohol, copper nitrate trihydrate and deionized water are mixed, heated to dissolve, polytetrafluoroethylene is added, and stirred to mix uniformly to obtain a spinning solution; (2) electrospinning the spinning solution to obtain polymer fibers; (3) placing the polymer fiber in a muffle furnace, heating the temperature to 280±10° C. at a heating rate of 2-3° C. / min, keeping the temperature for 2-3 hours, and cooling the temperature naturally to obtain pre-oxidized fiber; (4) The pre-oxidized fiber is placed in a tubular furnace under a protective gas atmosphere, firstly heated to 400-450°C at a heating rate of 2-3°C / min, then heated to 500-550°C at a heating rate of 0.8-1.2°C / min and kept warm for 1-2 h, then heated to 700-800°C at a heating rate of 2-3°C / min and kept warm for 2-3 h, and then cooled naturally to obtain a porous carbon-loaded copper metal shielding material.
10. A composite shielding body for generating a complex radiation environment for picosecond laser target shooting as claimed in claim 9, Features: In step (1), the mass ratio of polyvinyl alcohol, copper nitrate trihydrate and deionized water is 15-20:3-5:100; the mass ratio of polyvinyl alcohol to polytetrafluoroethylene is 1:1.8-2.2; In step (2), during electrospinning, the temperature is 40-50° C., the humidity is 40%-50%, the positive voltage is 20-25 KV, the negative voltage is -2-5 KV, the flow rate is 0.05-1 mm / min, and the receiving distance is 20-25 cm.
Citation Information
Patent Citations
Broadband transparent shielding material composite structure and composite glass and OCA back glue structure
CN109168315A
High-light-transmittance electromagnetic shielding film and preparation method thereof
CN113079683A
Sputtering shielding system and method for repetition frequency laser targeting
CN114485279A
Composite shielding material and preparation method thereof
CN116355586A
Honeycomb porous carbon nanofiber-high-entropy alloy composite wave-absorbing material as well as preparation method and application thereof
CN117306092A
Cited By
Stainless steel microsphere reinforced glass-based strong laser radiation resistant composite coating
CN120365776A
Grounding system for suppressing transient electromagnetic interference of laser targeting
CN122180058A
A grounding system for suppressing laser-targeting transient electromagnetic interference
CN122180058B