Austenitic stainless steel and method for producing austenitic stainless steel

By performing high-temperature primary heat treatment, low-temperature secondary heat treatment and controlled cold working in austenitic stainless steel, the problem of difficulty in balancing strength and ductility in solid materials was solved, achieving a tensile strength of more than 800MPa and a tensile strength of more than 35%. Elongation at break, suitable for components in high-pressure hydrogen environments.

CN118871602APending Publication Date: 2024-10-29NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026227.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-02-08
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

It is difficult to achieve cold working with a high cross-section reduction rate in solid materials using existing technology, resulting in austenitic stainless steel having poor performance in terms of high strength and ductility, making it difficult to achieve both.

Method used

Use a primary heat treatment at 1180 to 1280°C, followed by cold working with a cross-section reduction rate of more than 5% and less than 20%, and a secondary heat treatment at 1000 to 1180°C to ensure the miniaturization and refinement of Nb carbonitride and Nb nitride. Fully isolated to meet specific Nb content and grain diameter relationships to achieve high strength and ductility.

Benefits of technology

Through this method, a tensile strength of more than 800MPa and an elongation at break of more than 35% can be achieved in austenitic stainless steel, taking into account both strength and ductility, and is suitable for components in high-pressure hydrogen environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005032979670000141
    Figure BDA0005032979670000141
  • Figure BDA0005032979670000151
    Figure BDA0005032979670000151
  • Figure BDA0005032979670000171
    Figure BDA0005032979670000171
Patent Text Reader

Abstract

Provided is an austenitic stainless steel having excellent strength and ductility. The austenitic stainless steel has a chemical composition containing, in mass%, 0.005 to 0.060% of C, 0.20 to 1.20% of Si, 4.0 to 8.0% of Mn, 12.0 to 15.0% of Ni, 19.0 to 24.0% of Cr, 1.0 to 4.0% of Mo, 0.05 to 0.40% of Nb, 0.05 to 0.40% of V, 0.20 to 0.50% of N, 0.050% or less of Al, and the like, has a tensile strength of 800 MPa or more and an elongation at break of 35% or more, and satisfies the following formulae (1) and (2): 0.7 * Nb < = [Nb] < = 0.30 (1) and 20 * [Nb] / D > = 0.050 (2). In formula (1) and formula (2), the value of the Nb content of the chemical composition represented by mass% is substituted at "Nb", the value of the Nb amount analyzed in the form of an electrolytic extraction residue represented by mass% is substituted at "[Nb]", and the value of the crystal grain diameter represented by [mu] m is substituted at "D".
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an austenitic stainless steel and a method for producing the austenitic stainless steel. Background Art

[0002] In recent years, research on the practical application of transportation equipment that uses hydrogen as energy to replace fossil fuels has been advancing. For example, fuel cell vehicles that run on hydrogen as fuel and hydrogen refueling stations that supply hydrogen to fuel cell vehicles are being developed.

[0003] When stainless steel is used in fuel cell vehicles and hydrogen refueling stations, stainless steel is used in high-pressure hydrogen environments. In addition, lightweight fuel cell vehicles, miniaturization of hydrogen refueling stations, and high-pressure operation of hydrogen refueling stations are sought. Therefore, high strength is required for stainless steel used in fuel cell vehicles and hydrogen refueling stations.

[0004] International Publication No. 2012 / 132992 discloses a high-strength austenitic stainless steel for high-pressure hydrogen. International Publication No. 2017 / 056619 discloses an austenitic stainless steel having excellent strength, ductility and weldability. Japanese Patent Publication No. 2014-47420 discloses an austenitic stainless steel for a nuclear reactor that exhibits excellent strength in a nuclear reactor water temperature region and has excellent SCC resistance and weldability.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2012 / 132992

[0008] Patent Document 2: International Publication No. 2017 / 056619

[0009] Patent Document 3: Japanese Patent Application Publication No. 2014-47420 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] Various components are used in hydrogen refueling stations. In the past, piping made of steel pipes was widely used among the components used in hydrogen refueling stations. However, in recent years, high strength is required not only for piping but also for various components. In addition to piping, the application of austenitic stainless steel is also being studied. Such components include solid components. Therefore, even if it is a solid material, it is hoped that it can have both excellent strength and ductility like steel pipes.

[0012] International Publication No. 2012 / 132992 discloses that by cold working with a cross-sectional reduction rate of 20% or more after solution heat treatment, and then performing heat treatment again, austenitic stainless steel with a tensile strength of 800 MPa or more can be obtained. However, in the manufacturing process of solid materials, it is difficult to perform cold working with a high cross-sectional reduction rate.

[0013] An object of the present invention is to provide an austenitic stainless steel having excellent strength and ductility and a method for producing the austenitic stainless steel.

[0014] Solutions for solving problems

[0015] One embodiment of the present invention provides an austenitic stainless steel, wherein the chemical composition is, by mass%, C: 0.005-0.060%, Si: 0.20-1.20%, Mn: 4.0-8.0%, Ni: 12.0-15.0%, Cr: 19.0-24.0%, Mo: 1.0-4.0%, Nb: 0.05-0.40%, V: 0.05-0.40%, N: 0.20-0.50%, Al: 0.050% or less, Cu: 0-3.0%, Co: 0-0.50% Ca :0~0.0050%,B:0~0.0050%,W:0~0.10%,Ta:0~0.10%,the balance is Fe and impurities, P, S and O in the impurities are respectively P: 0.030% or less,S: 0.010% or less,and O: 0.015% or less,the tensile strength is 800MPa or more,the elongation at break is 35% or more,the Nb amount analyzed in the form of electrolytic extraction residue satisfies the following formula (1), and the Nb amount and grain size analyzed in the form of electrolytic extraction residue satisfy the following formula (2),

[0016] 0.7×Nb≤[Nb]≤0.30 (1)

[0017] 20×[Nb] / D≥0.050 (2)

[0018] In formula (1) and formula (2), the value of the Nb content of the chemical composition expressed in mass % is substituted in "Nb", the value of the Nb amount analyzed in the form of electrolytic extraction residue expressed in mass % is substituted in "[Nb]", and the value of the grain size expressed in μm is substituted in "D".

[0019] One embodiment of the present invention provides a method for manufacturing austenitic stainless steel, which is a method for manufacturing the above-mentioned austenitic stainless steel, and the manufacturing method comprises:

[0020] A step of subjecting the steel material having the chemical composition to a primary heat treatment at 1180-1280° C.;

[0021] After the primary heat treatment, a step of cold working the steel material with a cross-sectional reduction rate of 5% or more and less than 20%; and

[0022] A process of performing a secondary heat treatment on the steel material at a temperature of 1000 to 1180° C. after the cold working.

[0023] Effects of the Invention

[0024] According to the present invention, it is possible to obtain austenitic stainless steel having excellent strength and ductility. DETAILED DESCRIPTION

[0025] The present inventors have conducted various studies to solve the above-mentioned problems and have obtained the following findings (a) to (f).

[0026] (a) As a method for improving the strength of steel, there are solid solution strengthening and grain refinement using N. The austenitic stainless steel of this embodiment contains 0.20 to 0.50 mass % N, and the strength is improved by solid solution strengthening. If the grains are refined, the strength is further improved.

[0027] (b) As a method for refining the crystal grains, there is a method in which fine alloy carbonitrides or nitrides are precipitated during the final solution heat treatment, thereby suppressing the growth of crystal grains by means of the pinning effect. In order to generate fine carbonitrides or nitrides and refine the crystal grains of high nitrogen steel, it is effective to add Nb. However, in the conventional method, although Nb carbonitrides and Nb nitrides are precipitated, they are coarse and cannot fully exert the pinning effect.

[0028] (c) As a method for solving this problem, in International Publication No. 2012 / 132992, a method of sequentially performing solution heat treatment, cold working and secondary heat treatment is proposed. However, in the case of a solid material that is difficult to perform cold working with a high cross-sectional reduction rate, it is impossible to ensure strength and ductility by the same method.

[0029] (d) Therefore, as a primary heat treatment, a heat treatment before cold working is performed at a high temperature higher than the conventional solution heat treatment temperature. Thus, the alloying elements are further dissolved, and even if the strain is caused by cold working with a low cross-sectional reduction rate, the precipitation nuclei of Nb carbonitrides and Nb nitrides precipitated during the secondary heat treatment can be increased. Therefore, by cold working with a low cross-sectional reduction rate, Nb carbonitrides and Nb nitrides can be finely and more precipitated.

[0030] (e) If the effect of suppressing the growth of grains by pinning is the same, the grains will become relatively larger by making the temperature of the primary heat treatment and the secondary heat treatment high temperature. However, even when the grains are larger than the grains described in International Publication No. 2012 / 132992, high strength and ductility can be taken into account by making the amount of Nb carbonitrides and Nb nitrides and the size of the grains satisfy the prescribed relationship. Specifically, by making the amount of Nb analyzed in the form of electrolytic extraction residue satisfy the following formula (1) and making the amount of Nb analyzed in the form of electrolytic extraction residue and the grain diameter satisfy the following formula (2), it is possible to take into account high strength and ductility by utilizing the superposition effect of grain refinement and precipitation strengthening.

[0031] 0.7×Nb≤[Nb]≤0.30 (1)

[0032] 20×[Nb] / D≥0.050 (2)

[0033] In formula (1) and formula (2), the value of the Nb content expressed in mass % is substituted in "Nb", the value of the Nb amount expressed in mass % obtained by analysis in the form of electrolytic extraction residue is substituted in "[Nb]", and the value of the grain size expressed in μm is substituted in "D".

[0034] (f) It is further preferred that the secondary heat treatment be performed at a temperature of 1050 to 1160° C. By performing the secondary heat treatment in a temperature range near the precipitation peak of Nb carbonitride or Nb nitride, more Nb carbonitride or Nb nitride can be precipitated in a short time.

[0035] The present invention has been accomplished based on the above findings. Hereinafter, an austenitic stainless steel and a method for producing the austenitic stainless steel according to an embodiment of the present invention will be described in detail.

[0036] [Chemical formula composition]

[0037] The austenitic stainless steel according to one embodiment of the present invention has the chemical composition described below. In the following description, "%" of the content of an element represents mass %.

[0038] C: 0.005~0.060%

[0039] Carbon (C) is an element that helps stabilize austenite. In addition, C can generate Nb carbonitrides, which also helps ensure strength. In order to fully obtain this effect, the C content needs to be 0.005% or more. If the C content is too high, excess Nb carbonitrides will be generated, and the ductility of the steel will decrease. Therefore, the C content needs to be 0.060% or less. The lower limit of the C content is preferably 0.010%, and more preferably 0.020%. The upper limit of the C content is preferably 0.050%, and more preferably 0.040%.

[0040] Si: 0.20~1.20%

[0041] Silicon (Si) is an element that is effective as a deoxidizer and is an element that helps improve corrosion resistance. In order to fully obtain this effect, the Si content needs to be 0.20% or more. However, if the Si content is too high, the stability of the austenite structure will be reduced and the ductility of the steel will be reduced. Therefore, the Si content is 0.20-1.20%. The lower limit of the Si content is preferably 0.25%, and more preferably 0.30%. The upper limit of the Si content is preferably 1.10%, and more preferably 1.00%.

[0042] Mn: 4.0~8.0%

[0043] Manganese (Mn) is an element that helps deoxidation during manufacturing and also helps stabilize austenite. Mn also indirectly helps to increase the solubility of N and improve strength. If the Mn content is too low, these effects cannot be obtained. On the other hand, if the Mn content is too high, the ductility and hot workability of the steel will decrease. Therefore, the Mn content is 4.0 to 8.0%. The lower limit of the Mn content is preferably 4.5%, and more preferably 5.0%. The upper limit of the Mn content is preferably 7.5%, and more preferably 7.0%.

[0044] Ni: 12.0~15.0%

[0045] Nickel (Ni) is an element necessary to obtain stable austenite, which can increase the stacking fault energy and reduce the brittle sensitivity in a hydrogen-containing environment. In order to fully obtain this effect, the Ni content needs to be 12.0% or more. However, since Ni is an expensive element, if more Ni is contained, it will cause cost increase. Therefore, the Ni content is 12.0-15.0%. The lower limit of the Ni content is preferably 12.3%, and more preferably 12.5%. The upper limit of the Ni content is preferably 14.8%, and more preferably 14.5%.

[0046] Cr: 19.0~24.0%

[0047] Chromium (Cr) is an element necessary to ensure corrosion resistance in the use environment. Cr also indirectly helps to increase the solubility of N during manufacturing and improve strength. In order to fully obtain this effect, the Cr content needs to be 19.0% or more. However, if the Cr content is too high, the austenite structure will become unstable. Therefore, the Cr content is 19.0-24.0%. The lower limit of the Cr content is preferably 19.5%, and more preferably 20.0%. The upper limit of the Cr content is preferably 23.5%, and more preferably 23.0%.

[0048] Mo: 1.0~4.0%

[0049] Molybdenum (Mo) is an element that helps to improve corrosion resistance and strength in the use environment. In order to fully obtain this effect, the Mo content needs to be 1.0% or more. However, since Mo is an expensive element, if more Mo is contained, it will cause cost increase. In addition, if the Mo content is too high, the austenite structure will become unstable. Therefore, the Mo content is 1.0-4.0%. The lower limit of the Mo content is preferably 1.2%, and more preferably 1.5%. The upper limit of the Mo content is preferably 3.8%, and more preferably 3.5%.

[0050] Nb: 0.05~0.40%

[0051] Niobium (Nb) is an element that precipitates in the matrix in the form of fine carbonitrides and nitrides, which helps to improve strength. In order to fully obtain this effect, the Nb content needs to be 0.05% or more. However, if the Nb content is too high, the ductility of the steel will decrease. Therefore, the Nb content is 0.05-0.40%. The lower limit of the Nb content is preferably 0.10%, and more preferably 0.15%. The upper limit of the Nb content is preferably 0.35%, and more preferably 0.30%.

[0052] The Nb content here refers to the total amount of Nb contained in the austenitic stainless steel. That is, it refers to the sum of the amount of Nb dissolved in the matrix and the amount of Nb existing in the form of precipitates. In addition, in this embodiment, on the basis of the Nb content, the amount of Nb existing in the form of precipitates, that is, the amount of Nb analyzed in the form of electrolytic extraction residue, needs to be within a specified range.

[0053] V: 0.05~0.40%

[0054] Vanadium (V) is an element that precipitates in the matrix in the form of fine carbonitrides and nitrides, which helps to improve strength. In order to fully obtain this effect, the V content needs to be 0.05% or more. However, if the V content is too high, the ductility of the steel will decrease. Therefore, the V content is 0.05-0.40%. The lower limit of the V content is preferably 0.10%, and more preferably 0.15%. The upper limit of the V content is preferably 0.35%, and more preferably 0.30%.

[0055] N: 0.20~0.50%

[0056] Nitrogen (N) is dissolved in the matrix and contributes to high strength, and forms fine carbonitrides and nitrides with Nb and the like, which contribute to high strength. N is also an element that contributes to the stabilization of the austenite structure. In order to fully obtain these effects, the N content needs to be 0.20% or more. However, if the N content is too high, the hot workability during manufacturing will be reduced, and the precipitates of Nb will precipitate excessively, reducing the ductility of the steel. Therefore, the N content is 0.20 to 0.50%. The lower limit of the N content is preferably 0.23%, and more preferably 0.25%. The upper limit of the N content is preferably 0.48%, and more preferably 0.45%.

[0057] Al: 0.050% or less

[0058] Aluminum (Al) is contained as a deoxidizer like Si. However, if the Al content is too high, the cleanliness of the steel will decrease and the hot workability will decrease. Therefore, the Al content is 0.050% or less. The Al content is preferably 0.040% or less, and more preferably 0.030% or less. In addition, there is no need to specifically limit the lower limit of the Al content, but an extreme reduction will lead to an increase in steelmaking costs. Therefore, the lower limit of the Al content is preferably 0.005%, and more preferably 0.010%.

[0059] Cu: 0-3.0%

[0060] Copper (Cu) is an optional added element and may not be contained. Cu stabilizes austenite structure. Cu also improves the strength of steel by solid solution strengthening. As long as a small amount of Cu is contained, this effect can be obtained to some extent. However, Cu is an expensive element, so if more Cu is contained, it will cause cost increase. In addition, if the Cu content is too high, the ductility of the steel will decrease. Therefore, the Cu content is 0 to 3.0%. The lower limit of the Cu content is preferably 0.01%, and more preferably 0.10%. The upper limit of the Cu content is preferably 2.5%, and more preferably 2.0%.

[0061] Co: 0~0.50%

[0062] Cobalt (Co) is an optional added element and may not be contained. Co stabilizes the austenite structure. Co also improves the strength of steel by solid solution strengthening. As long as a small amount of Co is contained, this effect can be achieved to some extent. However, Co is an expensive element, so if more Co is contained, it will cause cost increase. Therefore, the Co content is 0 to 0.50%. The lower limit of the Co content is preferably 0.01%, and more preferably 0.10%. The upper limit of the Co content is preferably 0.30%, and more preferably 0.20%.

[0063] Ca: 0~0.0050%

[0064] Calcium (Ca) is an optional added element and may not be contained. Ca inhibits solidification cracking during steel casting. This effect can be achieved to some extent as long as a small amount of Ca is contained. However, if the Ca content is excessive, the hot workability of the steel will decrease. Therefore, the Ca content is 0 to 0.0050%. The lower limit of the Ca content is preferably 0.0001%, and more preferably 0.0005%. The upper limit of the Ca content is preferably 0.0040%, and more preferably 0.0030%.

[0065] B: 0~0.0050%

[0066] Boron (B) is an optional added element and may not be contained. B improves the strength of steel by refining the precipitates and thus the grains. This effect can be achieved to some extent as long as a small amount of B is contained. However, if the B content is excessive, the hot workability of the steel will decrease. Therefore, the B content is 0 to 0.0050%. The lower limit of the B content is preferably 0.0001%, and more preferably 0.0005%. The upper limit of the B content is preferably 0.0030%, and more preferably 0.0020%.

[0067] W: 0~0.10%

[0068] Tungsten (W) is an optional added element and may not be contained. W increases the strength of steel. As long as a small amount of W is contained, this effect can be obtained to some extent. However, even if tungsten (W) is contained excessively, the effect will be saturated. Therefore, the W content is 0 to 0.10%. The lower limit of the W content is preferably 0.01%, and more preferably 0.02%. The upper limit of the W content is preferably 0.08%, and more preferably 0.06%.

[0069] Ta: 0~0.10%

[0070] Tantalum (Ta) is an optional added element and may not be contained. Ta increases the strength of steel. As long as a small amount of Ta is contained, this effect can be obtained to some extent. However, even if tantalum (Ta) is contained excessively, the effect will be saturated. Therefore, the Ta content is 0 to 0.10%. The lower limit of the Ta content is preferably 0.001%, and more preferably 0.002%. The upper limit of the Ta content is preferably 0.08%, and more preferably 0.06%.

[0071] The balance of the chemical composition of the austenitic stainless steel of this embodiment is Fe and impurities. Impurities here refer to elements mixed from ores and scraps used as raw materials for steel, or elements mixed from the environment of the manufacturing process, etc. In this embodiment, the contents of P, S, and O in particular among the impurities are limited as follows.

[0072] P: 0.030% or less

[0073] Phosphorus (P) is contained in steel as an impurity. If the P content is too high, the hot workability during manufacturing will decrease. Therefore, the P content is 0.030% or less. The P content is preferably 0.025% or less, and more preferably 0.020% or less.

[0074] S: 0.010% or less

[0075] Sulfur (S) is contained in steel as an impurity. If the S content is too high, the hot workability during manufacturing will decrease. Therefore, the S content is 0.010% or less. The S content is preferably 0.005% or less, and more preferably 0.002% or less.

[0076] O: 0.015% or less

[0077] Oxygen (O) is contained in steel as an impurity. If the O content is too high, the hot workability during manufacturing will decrease, the cleanliness of the steel will deteriorate, and the ductility will decrease. Therefore, the O content is 0.015% or less. The O content is preferably 0.010% or less, and more preferably 0.005% or less.

[0078] [Analysis of Nb content and steel structure obtained as electrolytic extraction residue]

[0079] In the austenitic stainless steel of the present embodiment, the Nb amount analyzed as an electrolytic extraction residue satisfies the following formula (1), and the Nb amount analyzed as an electrolytic extraction residue and the grain size satisfy the following formula (2).

[0080] 0.7×Nb≤[Nb]≤0.30 (1)

[0081] 20×[Nb] / D≥0.050 (2)

[0082] In formula (1) and formula (2), the value of the Nb content expressed in mass % is substituted in "Nb", the value of the Nb amount expressed in mass % obtained by analysis in the form of electrolytic extraction residue is substituted in "[Nb]", and the value of the grain size expressed in μm is substituted in "D".

[0083] In the austenitic stainless steel of the present embodiment, the amount of Nb analyzed in the form of electrolytic extraction residue is more than 0.7 times the Nb content of the billet and less than 0.30 mass %. The Nb contained in the billet is precipitated as fine carbonitrides and nitrides during the solution heat treatment. The finely precipitated Nb carbonitrides and Nb nitrides will increase the strength of the steel. In order to obtain this effect, it is necessary to make the amount of Nb precipitated in the form of carbonitrides and nitrides, that is, the amount of Nb analyzed in the form of electrolytic extraction residues, more than 0.7 times the Nb content of the base material. However, if the amount of Nb analyzed in the form of electrolytic extraction residues is excessive, the ductility of the steel will decrease. Therefore, the upper limit of the amount of Nb analyzed in the form of electrolytic extraction residues is 0.30 mass %. The lower limit of the amount of Nb analyzed in the form of electrolytic extraction residues is more preferably 0.8 times the amount of Nb in the billet. The upper limit of the amount of Nb analyzed as an electrolytic extraction residue is more preferably 0.28 mass %, and further preferably 0.25 mass %.

[0084] In order to achieve both strength and excellent ductility, it is effective to use Nb carbonitrides and Nb nitrides to refine the grains. When achieving both strength and ductility, the Nb amount and grain size obtained by analyzing the extracted residue need to satisfy formula (2). The value on the left side of formula (2) is more preferably 0.060 or more, and more preferably 0.080 or more.

[0085] The amount of Nb analyzed as an electrolytic extraction residue can be adjusted by the Nb content and N content of the billet and the manufacturing conditions such as heat treatment. Specifically, the higher the Nb content and N content of the billet, the higher the amount of Nb analyzed as an electrolytic extraction residue. The manufacturing conditions will be described later.

[0086] The amount of Nb obtained by analyzing the electrolytic extraction residue is measured as follows. A test piece of a specified size is collected from austenitic stainless steel. A 10% acetylacetone-1% tetramethylammonium chloride / methanol solution is used as the electrolyte and constant current electrolysis is performed at a current density of 20 to 25 mA / cm 2 The test piece was dissolved at an anodic temperature to extract carbonitride and nitride as residue. The extracted residue was acid-lyzed and then subjected to ICP (high frequency inductively coupled plasma) emission spectrometry to measure the mass of Nb in the residue.

[0087] The grain diameter can be measured by the intercept method.

[0088] The grain size of the austenitic stainless steel of the present embodiment is preferably 20.0 μm or more. According to the austenitic stainless steel of the present embodiment, even when it is difficult to make the grain size less than 20.0 μm, both strength and ductility can be achieved. The lower limit of the grain size is more preferably 25.0 μm, and more preferably 30.0 μm. The upper limit of the grain size is preferably 60.0 μm.

[0089] [Mechanical properties]

[0090] The tensile strength of the austenitic stainless steel of the present embodiment is 800 MPa or more. The tensile strength of the austenitic stainless steel of the present embodiment is preferably 830 MPa or more, and more preferably 850 MPa or more.

[0091] The elongation at break of the austenitic stainless steel of the present embodiment is 35% or more. The elongation at break of the austenitic stainless steel of the present embodiment is preferably 38% or more, and more preferably 40% or more.

[0092] The austenitic stainless steel of the present embodiment is preferably a solid material (solid steel). "Solid material" herein refers to a member other than hollow members such as steel pipes. The austenitic stainless steel of the present embodiment is more preferably round steel, and is further preferably round steel with an outer diameter of more than 25 mm. Solid material, in particular round steel with an outer diameter of more than 25 mm, is difficult to manufacture by cold working with a higher cross-sectional reduction rate. The austenitic stainless steel of the present embodiment can take both strength and ductility into account even when it is difficult to implement cold working with a higher cross-sectional reduction rate. The lower limit of the outer diameter of the austenitic stainless steel of the present embodiment when it is round steel is further preferably 28 mm, further preferably 30 mm, and further preferably 33 mm.

[0093] The austenitic stainless steel of the present embodiment is preferably used as a material for equipment for storing or transporting high-pressure hydrogen gas or liquid hydrogen.

[0094] [Manufacturing method]

[0095] In the present embodiment, in order to precipitate fine Nb carbonitrides and Nb nitrides, the following primary heat treatment, cold working, and secondary heat treatment are performed in this order.

[0096] The primary heat treatment is carried out at a temperature above 1180°C so that the Nb carbonitrides and Nb nitrides generated in the process before the primary heat treatment such as hot working are fully dissolved. On the other hand, when the temperature of the primary heat treatment exceeds 1280°C, the grains will be extremely coarsened. The lower limit of the temperature of the primary heat treatment is preferably 1200°C. The upper limit of the temperature of the primary heat treatment is preferably 1260°C. In the following, for convenience, the temperature of the primary heat treatment is set to "T1 (°C)". The holding time of the primary heat treatment is preferably 1 to 20 minutes, and more preferably 1 to 10 minutes. In addition, the steel after the primary heat treatment is expected to be rapidly cooled, and ideally water-cooled.

[0097] After Nb carbonitride and Nb nitride are fully dissolved in the primary heat treatment, cold working and secondary heat treatment are performed, thereby enabling precipitation of fine Nb carbonitride and Nb nitride. In the present embodiment, since the cross-sectional reduction rate of cold working is reduced, it is necessary to preliminarily dissolve more Nb carbonitride and Nb nitride in the primary heat treatment. Since the Nb carbonitride and Nb nitride generated in hot working are coarse, they will not contribute to the miniaturization of grains achieved by the pinning effect. In addition, if the Nb carbonitride and Nb nitride generated in hot working are not fully dissolved and remain, it is more difficult to introduce strain in cold working.

[0098] Next, in order to increase the precipitation nuclei of Nb carbonitride and Nb nitride, cold working with a cross-sectional reduction rate of more than 5% and less than 20% is implemented. The higher the cross-sectional reduction rate, the more precipitation nuclei there are, and finer Nb carbonitrides and Nb nitrides will be precipitated during the secondary heat treatment. If the cross-sectional reduction rate of cold working is too low, fine Nb carbonitrides and Nb nitrides will not be precipitated during the secondary heat treatment, and the effect of grain refinement achieved by the pinning effect cannot be fully obtained. On the other hand, in the case where austenitic stainless steel is a thick-walled solid material, it is difficult to implement cold working with a cross-sectional reduction rate of more than 20%. The lower limit of the cross-sectional reduction rate of cold working is preferably 8%, and more preferably 10%. The upper limit of the cross-sectional reduction rate of cold working is preferably 18%, and more preferably 15%.

[0099] Finally, in order to remove the strain caused by cold working and precipitate fine Nb carbonitrides and Nb nitrides, a secondary heat treatment is performed at a temperature of 1000 to 1180° C. Hereinafter, for convenience, the heat treatment temperature in the secondary heat treatment is referred to as “T2 (° C.)”.

[0100] T2 is preferably 1050-1160°C. By performing a secondary heat treatment in a temperature range near the precipitation peaks of Nb carbonitrides and Nb nitrides, more Nb carbonitrides and Nb nitrides can be precipitated in a short time. The lower limit of T2 is more preferably 1080°C. The upper limit of T2 is more preferably 1120°C. The holding time of the secondary heat treatment is preferably 1-20 minutes, and more preferably 1-15 minutes. The steel after the secondary heat treatment is preferably quenched, and more preferably water-cooled.

[0101] Austenitic stainless steel and a method for producing austenitic stainless steel according to an embodiment of the present invention have been described above. According to this embodiment, austenitic stainless steel having excellent strength and ductility can be obtained.

[0102] Example

[0103] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0104] Steel ingots obtained by laboratory casting of steel grades A to J having the chemical composition shown in Table 1 were hot forged and hot rolled to produce plates with a thickness of 20 mm. Thereafter, a primary heat treatment was carried out at a temperature T1 (°C) shown in Table 2. The cooling after the primary heat treatment was water cooling. Thereafter, cold working with a cross-sectional reduction rate shown in Table 2 was performed. Thereafter, a secondary heat treatment was carried out at a temperature T2 (°C) shown in Table 2. The holding time of the primary heat treatment was set to 1 to 10 minutes, and the holding time of the secondary heat treatment was set to 1 to 15 minutes.

[0105] [Residue Analysis]

[0106] A test piece of 10 mm square and 30 mm long was collected from each test material, and the amount of Nb analyzed as an electrolytic extraction residue was measured according to the above method.

[0107] [Grain diameter]

[0108] Five test pieces were cut from each test material so that the cross section (T cross section) perpendicular to the rolling direction became the observation surface, mirror polished, corroded, and observed under an optical microscope. For each test piece, three viewing fields were observed at a magnification of 100 times, and the average grain size of each of the five test pieces was obtained by the intercept method, and then the average value was obtained as the grain size.

[0109] [Tensile test]

[0110] From each test material, a round bar tensile test piece based on JIS Z 2241 (2011) with a parallel portion diameter of 6 mm and a parallel portion length of 30 mm was collected and subjected to a tensile test at room temperature. The tensile test piece was collected from the center of the thickness direction of the plate so that the length direction of the test piece was parallel to the rolling direction. The tensile test was carried out using a method based on JIS Z 2241 (2011) to determine the tensile strength (MPa) and elongation at break (%).

[0111] The results are shown in Table 2. In Table 2, "R" is the cross-sectional reduction rate of cold working, "[Nb]" is the amount of Nb analyzed in the form of electrolytic extraction residue, "D" is the grain size, "TS" is the tensile strength, "EL" is the elongation at break, F1 is the value of the left side of formula (1) (0.7×Nb), and F2 is the value of the left side of formula (2) (20×[Nb] / D).

[0112] [Table 1]

[0113]

[0114] [Table 2]

[0115] Table 2

[0116]

[0117] As shown in Table 2, the tensile strength of the test materials of test numbers 1 to 25 was 800 MPa or more, and the elongation at break was 35% or more.

[0118] Test numbers 26 and 27 are test materials that have not been subjected to a primary heat treatment. Although the test material of test number 26 has sufficient ductility, the tensile strength is less than 800 MPa. It is believed that this is because formula (1) is not satisfied. On the other hand, although the test material of test number 27 has sufficient tensile strength, the elongation at break is less than 35%. It is believed that this is because formula (2) is not satisfied.

[0119] Although the test material of test number 28 has sufficient ductility, the tensile strength is less than 800MPa. It is believed that this is because formula (1) is not satisfied. It is believed that the reason for not satisfying formula (1) is that the temperature of the primary heat treatment is too low. The tensile strength and ductility of the test material of test number 29 are both low. It is believed that this is because formula (2) is not satisfied. It is believed that the reason for not satisfying formula (2) is that the temperature of the primary heat treatment is too high.

[0120] The tensile strength and ductility of the test material of test number 30 were both low. This is believed to be because the equations (1) and (2) were not satisfied. This is believed to be because the temperature of the secondary heat treatment was too high.

[0121] The test material of test number 31 has sufficient tensile strength, but the elongation at break is less than 35%. This is believed to be because the amount of Nb analyzed as an electrolytic extraction residue is too high. The reason why the amount of Nb analyzed as an electrolytic extraction residue is too high is that the temperature of the primary heat treatment is low relative to the Nb content of the billet, and the carbides and carbonitrides generated by hot working, etc. are not fully dissolved.

[0122] The tensile strength and ductility of the test material of test number 32 are both low. This is believed to be due to the low Nb content of the blank. The tensile strength and ductility of the test material of test number 33 are both low. This is believed to be due to the low N content of the blank.

[0123] Test Nos. 34 to 36 are test materials that have not undergone primary heat treatment and cold working. The tensile strength of the test materials of Test Nos. 34 and 35 is low. The ductility of the test material of Test No. 36 is low. These test materials do not satisfy equations (1) and (2).

[0124] The above is an evaluation test conducted using a plate material. The same evaluation was performed on a test material of round steel of steel type A. Specifically, for round steel formed by hot extrusion of a steel ingot with an outer diameter of 150 mm, a primary heat treatment was performed at a temperature T1 (°C) shown in Table 3. The cooling after the primary heat treatment was water cooling. Thereafter, cold drawing correction was performed in a manner to achieve a cross-sectional reduction rate as shown in Table 3, and a solid material in the shape of a round steel with an outer diameter of 55 mm was produced. Thereafter, a secondary heat treatment was performed at a temperature T2 (°C) shown in Table 2. The holding time of the primary heat treatment was set to 1 to 10 minutes, and the holding time of the secondary heat treatment was set to 1 to 15 minutes. The results are shown in Table 3.

[0125] [Table 3]

[0126] Table 3

[0127]

[0128] As shown in Table 3, the tensile strength of the test materials of test numbers 51 to 56 is 800 MPa or more, and the elongation at break is 35% or more. On the other hand, the tensile strength of the test material of test number 57 is less than 800 MPa. It is believed that this is because the formula (1) is not satisfied. It is believed that the reason for not satisfying the formula (1) is that the primary heat treatment was not performed.

[0129] Although the embodiments of the present invention have been described above, the above embodiments are merely examples for implementing the present invention. Therefore, the present invention is not limited to the above embodiments, and the above embodiments can be appropriately modified and implemented within the scope of the invention.

Claims

1. An austenitic stainless steel having a chemical composition of C: 0.005-0.060% by mass, Si: 0.20-1.20%, Mn: 4.0-8.0%, Ni: 12.0-15.0%, Cr:19.0~24.0%、 Mo: 1.0-4.0%, Nb: 0.05-0.40%, V:0.05~0.40%、 N:0.20~0.50%、 Al: 0.050% or less, Cu: 0-3.0%, Co: 0~0.50% Ca: 0~0.0050%, B:0~0.0050%、 W:0~0.10%、 Ta: 0~0.10%, The balance is Fe and impurities. The P, S and O in the impurities are respectively P: 0.030% or less, S: 0.010% or less, and O: 0.015% or less, The tensile strength of the austenitic stainless steel is 800 MPa or more. The elongation at break is more than 35%, The amount of Nb analyzed in the form of electrolytic extraction residue satisfies the following formula (1): The Nb amount and grain size obtained by analyzing the electrolytic extraction residue satisfy the following formula (2): 0.7×Nb≤[Nb]≤0.30 (1) 20×[Nb] / D≥0.050 (2) In formula (1) and formula (2), the value of the Nb content of the chemical composition expressed in mass % is substituted in "Nb", the value of the Nb amount analyzed in the form of electrolytic extraction residue expressed in mass % is substituted in "[Nb]", and the value of the grain size expressed in μm is substituted in "D".

2. The austenitic stainless steel according to claim 1, wherein: The austenitic stainless steel is a solid material.

3. The austenitic stainless steel according to claim 2, wherein: The solid material is round steel.

4. The austenitic stainless steel according to claim 3, wherein: The austenitic stainless steel has an outer diameter of 25 mm or more.

5. The austenitic stainless steel according to any one of claims 1 to 4, wherein The chemical composition contains, in mass%, selected from Cu: 0.01-3.0%, Co: 0.01~0.50%, Ca: 0.0001~0.0050%, B:0.0001~0.0050%、 W: 0.01~0.10%, and Ta: One or more elements selected from the group consisting of 0.001 to 0.10%.

6. The austenitic stainless steel according to any one of claims 1 to 4, wherein The austenitic stainless steel is used as a material for equipment for storing or transporting high-pressure hydrogen gas or liquid hydrogen.

7. A method for producing austenitic stainless steel, which is a method for producing the austenitic stainless steel according to any one of claims 1 to 4, the method comprising: A step of subjecting the steel material having the chemical composition to a primary heat treatment at 1180-1280° C.; After the primary heat treatment, a step of cold working the steel material with a cross-sectional reduction rate of 5% or more and less than 20%; and A process of performing a secondary heat treatment on the steel material at a temperature of 1000 to 1180° C. after the cold working.

8. The method for producing austenitic stainless steel according to claim 7, wherein: The temperature of the secondary heat treatment is 1050-1160°C.