Liquid medicine

By adding specific metal elements and organic solvents to the chemical solution, and controlling the content of metal elements through LA-ICP-MS, the problems of pattern collapse, uneven coating and particle defects caused by the chemical solution in EUV lithography technology are solved, and the problem is improved. Quality and stability of semiconductor device manufacturing.

CN118871864APending Publication Date: 2024-10-29FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027341.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-01-10
Filing Date
2023-03-09
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the manufacturing process of semiconductor devices, existing chemical solutions, especially when using EUV lithography technology, are difficult to effectively suppress the problems of pattern collapse, uneven resist coating, resist residue and particle defects, affecting the quality and efficiency of the process. .

Method used

Use a liquid containing specific metal elements (Fe, Ni, Zn) and organic solvents, and control the content of metal elements in the liquid through laser ablation-inductively coupled plasma-mass spectrometry (LA-ICP-MS) to ensure I The value is in the range of 0.010 to 10.000, combined with specific filtration and refining processes, to optimize the composition and process of the medicinal solution.

Benefits of technology

It effectively suppresses defects and problems in the developer, rinse, pre-wet, resist cleaning and piping cleaning solutions, improves the stability and quality of the process, and ensures the integrity of the pattern and the uniformity of the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118871864A_ABST
    Figure CN118871864A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a chemical solution that, when used in a step in which an object to be contacted is brought into contact with the chemical solution, is not susceptible to the occurrence of predetermined defects in the object to be contacted. This chemical solution contains: an organic solvent; and metal-containing particles containing a metal element selected from the group consisting of Fe, Ni, and Zn, the chemical solution having an I value of 0.010 to 10.000 as determined by the method X. Method X: a sample is prepared by applying the chemical solution on a substrate, the surface of the sample is scanned with laser by laser ablation-inductively coupled plasma-mass spectrometry analysis to analyze the sample, and a map is acquired for each of the metal elements in which the scanning time is the laser in the horizontal axis and the ion detection intensity is the vertical axis. The ion detection intensities in the map are integrated in accordance with the scanning time to obtain an integrated ion detection intensity for each of the metal elements, the integrated ion detection intensities for each of the metal elements are integrated as a total integrated ion detection intensity, and the total integrated ion detection intensity is divided by the scanning area of the laser light to obtain the total integrated ion detection intensity. And obtaining an I value with the unit of count / mm < 2 > (count / mm < 2 >).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a medicinal liquid. Background Art

[0002] When manufacturing semiconductor devices through a wiring formation process including photolithography, water and / or a chemical solution containing an organic solvent is used as a pre-wetting liquid, a resist liquid (resist composition), a developer, a rinse liquid, a stripping liquid, a chemical mechanical polishing (CMP) slurry, a cleaning liquid after CMP, etc., or as a diluent thereof.

[0003] In recent years, due to the progress of photolithography technology, the miniaturization of patterns has been continuously developed. As a method for miniaturizing patterns, a method of shortening the wavelength of the exposure light source is used, and attempts have been made to form patterns using EUV (extreme ultraviolet light) with a shorter wavelength instead of the ultraviolet light, KrF excimer laser, ArF excimer laser, etc. that have been used so far as the exposure light source.

[0004] The patterning system using EUV or the like has been developed with the goal of achieving a resist pattern width of 10 to 15 nm, and the chemical solution used in this process is required to have a higher defect suppression performance.

[0005] The chemical solution may contain metal impurities including metal elements as impurities. As a method of removing the metal impurities from the chemical solution, filtration can be mentioned.

[0006] Patent Document 1 discloses a method for purifying a liquid (chemical solution) using a porous membrane of polyimide and / or polyamide-imide having continuous pores. It is also disclosed that iron (Fe) and zinc (Zn) can be removed from the chemical solution according to the method.

[0007] Previous technical literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2016-155121 Summary of the invention

[0010] Technical issues to be solved by the invention

[0011] The present inventors prepared a chemical solution with reference to the method described in Patent Document 1. When the method was used in a step of bringing an object into contact with the prepared chemical solution, it was found that defects were easily generated in the object and the level required recently was not achieved.

[0012] In addition, when the liquid is used for various purposes such as developer, rinse solution, resist cleaning solution and pipe cleaning solution, it is expected that the problem occurring in each purpose will not occur. For example, when the liquid is used as developer or rinse solution, it is expected to suppress the pattern collapse of the formed resist pattern. In addition, when the liquid is used as pre-wet liquid, it is expected to suppress the uneven coating of the resist occurring on the pre-wet substrate. In addition, when the liquid is used as resist cleaning solution, it is expected to suppress the generation of resist residue. In addition, when used as pipe cleaning solution, it is expected to suppress the generation of particle defects on the surface of the substrate supplied with the composition by the pipe after cleaning.

[0013] Therefore, the object of the present invention is to provide a chemical solution, which, when used in a process of bringing an object into contact with the chemical solution, is less likely to cause defects in the object, and can be used as at least one of a developer, a rinse solution, a pre-wet solution, a resist cleaning solution and a pipe cleaning solution, and when used as a developer or a rinse solution, suppresses pattern collapse, when used as a pre-wet solution, suppresses uneven coating of the resist, when used as a resist cleaning solution, suppresses the generation of resist residues, and when used as a pipe cleaning solution, suppresses the generation of particle defects on the surface of a substrate to which the composition is supplied through a cleaned pipe.

[0014] Means for solving technical problems

[0015] The present inventors have conducted intensive research to solve the above-mentioned problems, and have finally completed the present invention. Specifically, they have found that the above-mentioned problems can be solved by the following structure.

[0016] [1] A medicinal solution comprising:

[0017] Organic solvents; and

[0018] containing metal particles comprising a metal element selected from the group consisting of Fe, Ni and Zn,

[0019] The I value of the drug solution obtained by method X is 0.010 to 10.000.

[0020] Method X: The above-mentioned liquid medicine is coated on a substrate to prepare a test object, and the surface of the test object is analyzed by scanning the laser using laser ablation-inductively coupled plasma-mass spectrometry. A graph with the horizontal axis being the laser scanning time and the vertical axis being the ion detection intensity is obtained for each of the above-mentioned metal elements, and the above-mentioned ion detection intensities in the above-mentioned graph are accumulated according to the above-mentioned scanning time to obtain the accumulated ion detection intensity of each of the above-mentioned metal elements, and the accumulated ion detection intensities of each of the above-mentioned metal elements are summed up and set as the total accumulated ion detection intensity, and the total accumulated ion detection intensity is divided by the scanning area of ​​the laser to obtain the unit of counts / mm 2 (count / mm2 )’s I value.

[0021] [2] The drug solution according to [1], wherein:

[0022] The chemical solution is one selected from the group consisting of a developer, a rinser, a pre-wet solution, a resist cleaning solution, and a pipe cleaning solution.

[0023] [3] The drug solution according to [1] or [2], wherein:

[0024] The organic solvent includes butyl acetate, 4-methyl-2-pentanol, cyclohexanone, propylene glycol monomethyl ether acetate or isopropyl alcohol.

[0025] [4] The drug solution according to any one of [1] to [3], wherein

[0026] The above-mentioned liquid is a developer.

[0027] The organic solvent is selected from the group consisting of butyl acetate and 4-methyl-2-pentanol, or

[0028] The organic solvent is a mixture of propylene glycol monomethyl ether acetate and a liquid organic acid.

[0029] [5] The drug solution according to any one of [1] to [3], wherein

[0030] The above-mentioned liquid is a flushing liquid.

[0031] The organic solvent is selected from the group consisting of butyl acetate, 4-methyl-2-pentanol and isopropyl alcohol.

[0032] [6] The drug solution according to any one of [1] to [3], wherein

[0033] The above-mentioned liquid medicine is a pre-wetting liquid.

[0034] The organic solvent is selected from the group consisting of cyclohexanone, propylene glycol monomethyl ether acetate and isopropyl alcohol.

[0035] [7] The drug solution according to any one of [1] to [3], wherein

[0036] The above-mentioned liquid is a resist cleaning liquid.

[0037] The above organic solvent is propylene glycol monomethyl ether acetate.

[0038] [8] The drug solution according to any one of [1] to [3], wherein

[0039] The above liquid is a pipe cleaning liquid.

[0040] The organic solvent is selected from the group consisting of butyl acetate, 4-methyl-2-pentanol, cyclohexanone, isopropyl alcohol and propylene glycol monomethyl ether acetate.

[0041] Effects of the Invention

[0042] According to the present invention, a chemical solution can be provided. When the chemical solution is used in a process of bringing an object into contact with the chemical solution, the object is less likely to have defects, and the chemical solution can be used as at least one of a developer, a rinse solution, a pre-wet solution, a resist cleaning solution, and a pipe cleaning solution. When used as a developer or a rinse solution, pattern collapse is suppressed. When used as a pre-wet solution, uneven coating of the resist is suppressed. When used as a resist cleaning solution, generation of resist residues is suppressed. When used as a pipe cleaning solution, generation of particle defects on the surface of a substrate to which a composition is supplied through a cleaned pipe is suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 Schematic cross-sectional view illustrating an example of a method of implementing laser ablation-inductively coupled plasma-mass spectrometry in method X. DETAILED DESCRIPTION

[0044] Hereinafter, the present invention will be described in detail.

[0045] Although the description of the components described below may be made based on typical embodiments of the present invention, the present invention is not limited to such embodiments.

[0046] The meaning of each description in this specification is shown below.

[0047] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0048] In this specification, Fe, Ni, and Zn are element symbols, and represent iron, nickel, and zinc, respectively.

[0049] In this specification, "radiation" refers to, for example, far ultraviolet rays, extreme ultraviolet rays (EUV), X-rays, or electron beams. In addition, in the present invention, light refers to actinic rays or radiation. Unless otherwise specified, "exposure" in the present invention includes not only exposure by far ultraviolet rays, X-rays, or EUV, but also drawing by particle beams such as electron beams or ion beams.

[0050] <Medicine>

[0051] The chemical solution of the present invention comprises: an organic solvent; and metal-containing particles containing a metal element selected from the group consisting of Fe, Ni and Zn, wherein the chemical solution has an I value of 0.010 to 10.000 obtained by method X described in detail below.

[0052] Hereinafter, after explaining the above-mentioned organic solvent and metal-containing particles, the value I and the method X will be explained in detail.

[0053] In addition, hereinafter, in the case of a process for bringing an object to be contacted into contact with a chemical solution, a case where the object to be contacted is less likely to be defective is also referred to as “less likely to be defective”.

[0054] [Organic solvents]

[0055] The drug solution of the present invention contains an organic solvent.

[0056] In this specification, an organic solvent refers to a liquid organic compound contained in an amount of more than 10,000 ppm by mass of each component relative to the total mass of the above-mentioned drug solution. That is, in this specification, a liquid organic compound contained in an amount of more than 10,000 ppm by mass relative to the total mass of the above-mentioned drug solution is equivalent to an organic solvent.

[0057] In this specification, the term "liquid" means liquid at 25°C and atmospheric pressure.

[0058] The drug solution of the present invention preferably contains an organic solvent as a main component.

[0059] The organic solvent as the main component in the drug solution means that the content of the organic solvent in the drug solution is 98.0 mass % or more, preferably more than 99.0 mass %, more preferably more than 99.90 mass %, and even more preferably more than 99.95 mass %, relative to the total mass of the drug solution. The upper limit is less than 100 mass %.

[0060] The organic solvent may be used alone or in combination of two or more. When two or more organic solvents are used, the total content is preferably within the above range.

[0061] There are no particular restrictions on the type of organic solvent, and a known organic solvent can be used. Examples of the organic solvent include alkylene glycol monoalkyl ether carboxylates, alkylene glycol monoalkyl ethers, alkyl lactates, alkyl alkoxypropionates, cyclic lactones (preferably having 4 to 10 carbon atoms), monoketone compounds that may have a ring (preferably having 4 to 10 carbon atoms), alkylene carbonates, alkyl alkoxy acetates, alkyl pyruvates, dialkyl sulfoxides, cyclic sulfones, dialkyl ethers, monohydric alcohols, diols, alkyl acetates, and N-alkylpyrrolidone.

[0062] The organic solvent is preferably selected from the group consisting of, for example, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), cyclohexanone (CHN), ethyl lactate (EL), propylene carbonate (PC), isopropyl alcohol (IPA), 4-methyl-2-pentanol (MIBC), butyl acetate (nBA), propylene glycol monoethyl ether, propylene glycol monopropyl ether, methyl methoxypropionate, cyclopentanone, γ-butyrolactone, diisoamyl ether, isoamyl acetate, dimethyl sulfoxide, N-methylpyrrolidone, diethylene glycol, ethylene glycol, dipropylene glycol, propylene glycol, ethylene carbonate, sulfolane, cycloheptanone, 2-heptanone and liquid organic acids (for example, formic acid, acetic acid, propionic acid, butyric acid and lactic acid (racemic)). At least one.

[0063] Examples of using two or more organic solvents include a combination of PGMEA and PGME, a combination of PGMEA and PC, and a combination of PGMEA and one or more selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid, and lactic acid (racemic form).

[0064] In addition, the type and content of the organic solvent in the chemical solution can be measured using a gas chromatography-mass spectrometer.

[0065] [Containing metal particles]

[0066] The chemical solution of the present invention contains metal-containing particles containing a metal element selected from the group consisting of Fe, Ni, and Zn.

[0067] From the metal-containing particles, ions derived from the metal-containing particles are detected by laser ablation-inductively coupled plasma-mass spectrometry, and an I value described in detail later is obtained.

[0068] The preferred method of manufacturing the liquid medicine will be described later, but the liquid medicine can be manufactured by refining the object to be purified containing the above-mentioned organic solvent and impurities. The metal-containing particles can be actively added in the manufacturing process of the liquid medicine, can be contained in the object to be purified, or can be metal-containing particles transferred from the liquid medicine manufacturing device during the manufacturing process of the liquid medicine (so-called contamination).

[0069] The metal-containing particles can be any metal element selected from the group consisting of Fe, Ni and Zn, and their form is not particularly limited. For example, they can be monomers of the above metal elements, compounds containing metal elements (hereinafter also referred to as "metal compounds"), or complexes thereof. In addition, the drug solution can contain a variety of metal-containing particles.

[0070] The metal-containing particles may contain two or more of the above-mentioned metal elements in one metal-containing particle.

[0071] The elements other than the above-mentioned metal elements contained in the metal compound are not particularly limited, and for example, other metal elements and non-metal elements can be cited. As other metal elements, aluminum (Al), titanium (Ti), chromium (Cr) and lead (Pb) can be cited. As non-metal elements, hydrogen (H), carbon (C), nitrogen (N), oxygen (O), sulfur (S) and phosphorus (P) can be cited, among which oxygen is preferred. As the form of oxygen atoms contained in the metal compound, although there is no particular limitation, it is more preferably an oxide of the metal element.

[0072] The above-mentioned composite is not particularly limited, and examples thereof include so-called core-shell particles having a monomer of a metal element and a metal compound covering at least a portion of the monomer of the above-mentioned metal element, solid solution particles containing a metal element and other elements, agglomerate particles of a monomer of a metal element and a metal compound, agglomerate particles of different types of metal compounds, and metal compounds whose composition changes continuously or intermittently from the surface of the particle to the center.

[0073] [I value]

[0074] The I value of the drug solution of the present invention obtained by the following method X is 0.010 to 10.000. The I value is a regulation indicating the amount of a predetermined metal element contained in the drug solution. The smaller the I value, the smaller the amount of the predetermined metal element.

[0075] Method X: A test object is prepared by coating a chemical solution on a substrate, and a surface of the test object is analyzed by scanning a laser using a laser ablation-inductively coupled plasma-mass spectrometry method. A graph with a horizontal axis representing the laser scanning time and a vertical axis representing the ion detection intensity is obtained for each of the above metal elements (Fe, Ni, and Zn). The ion detection intensity of the graph is accumulated according to the scanning time to obtain the accumulated ion detection intensity of each metal element. The accumulated ion detection intensity of each metal element is summed up and set as the total accumulated ion detection intensity. The total accumulated ion detection intensity is divided by the scanning area of ​​the laser to obtain a value in counts / mm 2 The I value of .

[0076] The I value is preferably 0.010 to 5.000, more preferably 0.010 to 2.500.

[0077] Hereinafter, method X will be described.

[0078] (Subject)

[0079] In method X, first, a chemical solution is applied on a substrate to prepare a specimen.

[0080] The substrate is preferably a substrate with a high degree of cleanliness on the substrate surface. As the substrate, a semiconductor substrate can be cited, and more specifically, a silicon wafer can be used. In addition, the size of the substrate is not particularly limited, and can be appropriately determined according to the style of the coating device for coating the chemical solution on the substrate, the style of the device for performing the analysis, and the amount of the chemical solution to be measured.

[0081] The method for applying the chemical solution is not particularly limited, and examples thereof include spin coating. As an apparatus for applying the chemical solution, for example, a coating and developing device can be used.

[0082] (LA-ICP-MS)

[0083] In method X, the specimen is analyzed by laser ablation-inductively coupled plasma-mass spectrometry (LASER-Ablation-Inductively Coupled Plasma-Mass Spectrometry, hereinafter also referred to as "LA-ICP-MS").

[0084] LA-ICP-MS is a method in which a laser is irradiated on the sample surface to melt and vaporize the sample surface, thereby generating gas or particles or a mixture thereof (hereinafter also referred to as vaporized products) originating from the sample surface; the vaporized products originating from the sample surface are introduced into an inductively coupled plasma-mass spectrometry (ICP-MS) unit to perform a quantitative analysis of the elements contained in the vaporized products originating from the sample surface.

[0085] According to LA-ICP-MS, even extremely small amounts of elemental components present on the surface of a test object can be analyzed.

[0086] The specific method for implementing LA-ICP-MS is not particularly limited, and examples thereof include: Figure 1 The analytical method shown.

[0087] Figure 1 This is a schematic cross-sectional view for explaining an example of a method for implementing LA-ICP-MS.

[0088] exist Figure 1 In the method shown, a carrier gas supply unit 38 and an analysis unit 36 ​​are connected to the container unit 33. The container unit 33 and the supply unit 38 are connected by a pipe 39, and the container unit 33 and the analysis unit 36 ​​are connected by a pipe 39.

[0089] The container portion 33 can accommodate the specimen 50 , and analysis is performed in a state where the entire specimen 50 is accommodated in the container portion 33 and a carrier gas is supplied from the carrier gas supply portion 38 into the container portion 33 .

[0090] Then, if Figure 1As shown in FIG. 5 , the surface 50a of the object 50 is irradiated with laser light La. Figure 1 , a state where the metal-containing particles 51 contained in the liquid medicine are irradiated with the laser light La is schematically shown. When the metal-containing particles 51 are irradiated with the laser light La, ablation occurs, and a vaporized product derived from the metal-containing particles 51, i.e., an analysis sample 51a, is generated. The generated analysis sample 51a moves to the analysis unit 36 ​​along with the carrier gas. The analysis sample 51a derived from the metal-containing particles 51 is analyzed by ICP-MS in the analysis unit 36.

[0091] By performing the irradiation of the laser light La while changing the position, that is, scanning the laser light La, and performing analysis by ICP-MS each time, a graph with the laser scanning time on the horizontal axis and the ion detection intensity on the vertical axis can be obtained for each metal element.

[0092] The irradiation of the laser light is preferably performed in a pulsed state. In the present invention, the irradiation of the laser light is performed under the laser light and conditions described later.

[0093] The analyzing unit 36 ​​will be described.

[0094] The analysis unit 36 ​​is a unit using the above-mentioned ICP-MS, and performs Figure 1 Mass spectrometry analysis of the analytical sample 51a described in .

[0095] In the analysis unit 36, the object to be measured is ionized by high-temperature plasma maintained by high-frequency electromagnetic induction, and the ions are detected by a mass spectrometer (mass spectrometer), thereby measuring the mass of the ions and the number of ions (ion detection intensity).

[0096] As the mass spectrometer, a known mass spectrometer can be used. Examples of the mass spectrometer include a time of flight mass spectrometer, a quadrupole mass spectrometer, and a magnetic field mass spectrometer, and a quadrupole mass spectrometer (QMS) is preferred.

[0097] The analysis unit 36 ​​can obtain, for example, a signal of the detected element ions (not shown) and a graph (not shown) with the horizontal axis representing the laser scanning time and the vertical axis representing the ion detection intensity. The concentration of the detected element corresponds to the ion detection signal intensity.

[0098] (Detection intensity diagram)

[0099] In the above method, by using LA-ICP-MS to analyze the surface of the object by laser scanning, a graph (hereinafter also referred to as a "detection intensity graph") with the laser scanning time on the horizontal axis and the ion detection intensity (unit: count) on the vertical axis can be obtained for each metal element. That is, the detection intensity graph C of Fe can be obtained. Fe , Ni detection intensity diagram C Ni And the detection intensity of Zn in Figure C Zn .

[0100] In addition, in this specification, it is assumed that the measurement is performed under the following conditions, and the detection intensity map C is obtained by the following processing: Fe , Detection intensity diagram C Ni And detection intensity map C Zn .

[0101] In addition, in the following, first, Fe, Ni and Zn are simultaneously analyzed in one sample by LA-ICP-MS and the detection intensity maps (C Fe , C Ni and C Zn ) method is described in detail.

[0102] - Preparation of specimens -

[0103] In the preparation of the specimen, a silicon wafer (manufactured by Shin-Etsu Semiconductor Co., Ltd., 12 inches) was used, and the amount of the chemical solution applied was set to 1 mL. The chemical solution was applied by spin coating, and the rotation speed during spin coating was set to 500 rpm.

[0104] -LA-ICP-MS measurement conditions-

[0105] The scanning area (analysis area) of the laser light was set to the entire surface of the silicon wafer.

[0106] The laser used was a pulsed laser with a wavelength of 260 nm and a pulse width of 290 femtoseconds and a fluence of 1 J / cm 2 , the oscillation frequency of the pulse laser was set to 10 kHz, and the irradiation diameter of the pulse laser was set to 10 μm.

[0107] The laser scans linearly at 100 mm / s. After scanning from one end of the silicon wafer to the other end, the laser scans in the opposite direction (from the other end to one end) from a position offset by 10 μm in a direction orthogonal to the scanning direction. This operation is repeated to scan the entire surface of the wafer.

[0108] Argon or helium was used as a carrier gas, and the carrier gas was supplied at 10 mL / min.

[0109] Argon gas was supplied to the plasma torch, and a high frequency current of 40.68 MHz and 1.3 kW was applied to generate plasma. A coaxial type atomizer was used, the flow rate of the atomizer was set to 0.94 L / min, and the supply amount of argon gas for cooling was set to 13 L / min.

[0110] The mass spectrometry unit uses a quadrupole mass spectrometer. The detection mode in the ion detector is set to the selected ion detection (SIM) mode, and the m / z of the detected ions is set to 56 (Fe), 58 (Ni) and 64 (Zn). The detection time (cycle time) for detecting each m / z ion once is set to 3 milliseconds. That is, a switching scan is performed to selectively detect several ion types (measured ion types) with different m / z in sequence. In the switching scan, the ion amount of several ion types with a specific m / z can be repeatedly measured in a short period of time, and a cycle in which multiple measured ion types as the measurement object are detected once is equivalent to the above-mentioned detection time. In addition, in the detection time, the time for detecting one measured ion type is called the counting time.

[0111] The measurement conditions can also be referred to BUNSEKI RIGAKU Vol.68, No.1, pp.1-7 (2019) by Yamashita et al. and J. Mass. Spectrom. Soc. Jpn Vol.67, No.5, pp.160-166 (2019) by Hirata et al.

[0112] In addition, for example, the ion detection intensity (unit: count) of the ion of m / z = 56 in the above-mentioned detection time can be calculated by multiplying the ion detection count rate (unit: count / second) detected in the counting time for detecting the ion of m / z = 56 by the above-mentioned detection time, and the value of the ion detection intensity corresponding to the ion detection intensity of m / z = 56 when only the ion of m / z = 56 is detected in the above-mentioned detection time can be calculated.

[0113] -Signal processing method-

[0114] Below, for obtaining the detection intensity map C Fe , Detection intensity diagram C Ni And detection intensity map C Zn The signal processing method is described below.

[0115] First, the silicon wafer without the chemical solution was measured using the above method to obtain a background image C of each m / z, where the horizontal axis is the laser scanning time and the vertical axis is the ion detection intensity. Bn In addition, the value of m / z is substituted into n. For example, the background image at m / z=56 is called background image C. B56 , background image C Bn A general term for the background map of each m / z measured.

[0116] In addition, the background image C Bn The average value of the ion detection intensity in is set as the background average value I Bnave , the background image C Bn The standard deviation of the ion detection intensity in is set as the standard deviation σ Bn In addition, for example, in the background image C B56 The average value of the ion detection intensity is called the background average value I B56ave , the standard deviation of the ion detection intensity is called the standard deviation σ B56 .

[0117] In addition, for example, background image C B56 The ion detection intensity (unit: count) in the above detection time is a value obtained by multiplying the ion detection count rate (unit: count / second) detected in the counting time for detecting ions of m / z=56 by the above detection time.

[0118] Then, through the above steps, in the process of obtaining the background image C Bn The chemical solution is applied to other wafers of the same type as the wafer to obtain the test object, and the above measurement is performed to obtain a mass spectrum with the m / z value at each detection time. Therefore, the ion detection intensity (unit: count) for each m / z is used as the vertical axis and the scanning time is used as the horizontal axis, thereby obtaining the detection intensity graph C before treatment. m / z=n In addition, the value of m / z is substituted into n. For example, the detection intensity map before processing at m / z=56 is called the detection intensity map before processing C. m / z=56 , Detection intensity map before treatment C m / z =n is the collective name of the detected intensity map before processing at each m / z measured.

[0119] In addition, for example, the detection intensity map C before processing m / z=56 The ion detection intensity (unit: count) in the above detection time is a value obtained by multiplying the ion detection count rate (unit: count / second) detected in the counting time for detecting ions of m / z=56 by the above detection time.

[0120] Here, the detection intensity map C Fe , Detection intensity diagram C Ni And detection intensity map C Zn By detecting the intensity map before treatment C m / z=n The following signal processing is performed to obtain the detection intensity map C. Fe The method is represented as an example to illustrate.

[0121] Iron (Fe) exists 54 Fe, 56 Fe,57 Fe and 58 Fe as a stable isotope, 56 The natural existence ratio of Fe is the largest. Here, when obtaining the detection intensity map C Fe When 56 The ions with m / z corresponding to Fe are taken as the detection objects. 56 Detection intensity of ions with m / z corresponding to Fe before treatment (Figure C) m / z=56 , and perform signal processing and analysis to obtain the detection intensity graph C Fe .

[0122] and 56 Fe corresponding to the pre-treatment detection intensity map C m / z=56 It may contain background and noise. Therefore, first, according to the pre-processing detection intensity map C m / z=56 , and the background average value I is subtracted B56ave Corrected image C m / z=56 .

[0123] Furthermore, in the correction diagram C after the above subtraction m / z=56 In the figure, the standard deviation σ is shown. B56 Signals with a detection intensity six times or more of that of ions 1 and 2 are considered to be signals generated by ions of m / z=56.

[0124] In the correction diagram C m / z=56 In each detection time of , if the signal is not considered to be generated by the ion of m / z=56, the ion detection intensity in the detection time is set to 0. m / z=56 The graph obtained by performing the above processing at each detection time is set as the detection intensity graph C Fe .

[0125] In addition, the detection intensity map C Fe This corresponds to a graph obtained by estimating the detection intensity of the ion of m / z=56 when only the ion of m / z=56 is detected.

[0126] Through the same signal processing as above, the detection intensity map C can also be obtained Ni And detection intensity map C Zn .

[0127] In addition, nickel (Ni) exists 58 You, 60 You, 61 You, 62 Ni and 64 Ni is a stable isotope. 58 Ni has the largest natural existence ratio, so when obtaining the detection intensity map C Ni When 58 Ions with m / z corresponding to Ni are detected.

[0128] In addition, zinc (Zn) exists 64 Zn, 66 Zn, 67 Zn, 68 Zn and 70 Zn as a stable isotope, 64 Zn has the largest natural abundance ratio, so when obtaining the detection intensity map C Zn When 64 The ions with m / z corresponding to Zn are detected.

[0129] (Calculation of I value)

[0130] According to the detection intensity map of each metal element (C Fe , C Ni and C Zn ) is used to illustrate the method of calculating the I value.

[0131] For each detection intensity map (C Fe , C Ni and C Zn ), the ion detection intensity (unit: count) is accumulated according to the scanning time to obtain the cumulative ion detection intensity (unit: count) of each metal element. That is, the cumulative ion detection intensity I of Fe can be obtained. Fe , Cumulative ion detection intensity I of Ni Ni and the cumulative ion detection intensity I of Zn Zn The above-mentioned accumulation means that all ion detection intensities in each figure are totaled within the scanning time.

[0132] Next, the cumulative ion detection intensity for each metal element is summed up and set as the total cumulative ion detection intensity (cumulative ion detection intensity I Fe , cumulative ion detection intensity I Ni and the cumulative ion detection intensity I Zn of the total value).

[0133] The I value can be obtained by dividing the above total cumulative ion detection intensity by the scanning area of ​​the laser. The unit of the I value is count / mm 2 .

[0134] In the above method, Fe, Ni and Zn are simultaneously analyzed in one sample by LA-ICP-MS to obtain the detection intensity maps (C Fe , C Ni and C Zn ) method has been described, but a method using individual subjects as follows is also possible.

[0135] That is, the same chemical solution can be applied to a plurality of substrates of the same type to prepare a plurality of test specimens, and one element can be analyzed for one test specimen by LA-ICP-MS to obtain the detection intensity map (C Fe , C Ni and C Zn ). For example, when only the ion of m / z=56 is used as the object for analysis of one of the above multiple samples by LA-ICP-MS, and the background and noise are removed according to the above method, a detection intensity graph C with the horizontal axis being the laser scanning time and the vertical axis being the ion detection intensity can be obtained. Fe In addition, the detection intensity map C is obtained by using the above method. Fe In the case of background image C B56 , background average value I B56ave and standard deviation σ B56 The values ​​obtained by analyzing the substrate without the chemical solution by LA-ICP-MS with only ions of m / z=56 as the target were used. The detection intensity graph C was obtained by analyzing other samples using the same procedure. Ni And detection intensity map C Zn .

[0136] [Other ingredients]

[0137] The chemical solution of the present invention may contain other components in addition to the above-mentioned components. Examples of other components include organic compounds other than organic solvents (particularly organic compounds having a boiling point of 300° C. or higher), water, and resins.

[0138] In addition, as other components, solid organic acids can be mentioned. Solid organic acids refer to organic acids that are solid at 25° C. and atmospheric pressure. Examples of solid organic acids include oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, glutaric acid, tartronic acid, malic acid, tartaric acid, glycolic acid, citric acid, and lactic acid (D-lactic acid or L-lactic acid).

[0139] The total content of other components is preferably 2% by mass or less, more preferably 1% by mass or less, and further preferably 0.1% by mass or less relative to the total mass of the drug solution. For example, the total content of other components is preferably more than 0% by mass relative to the total mass of the drug solution.

[0140] The total content of the solid organic acid is preferably 1% by mass or less, more preferably 0.001% by mass or less, and even more preferably 0.0001% by mass or less, relative to the total mass of the drug solution.

[0141] <Application of the drug solution>

[0142] The use of the medicinal solution of the present invention is not particularly limited.

[0143] Among them, the use of the chemical solution is preferably used in a semiconductor device manufacturing method (process). That is, it is preferred that the semiconductor device manufacturing method include a step of using the chemical solution of the present invention.

[0144] The above-mentioned chemical solution can also be used in any process for manufacturing semiconductor devices. Among them, the above-mentioned chemical solution is preferably used in a process including resist pattern formation. That is, it is preferred that the process of using the chemical solution of the present invention is included in the resist pattern formation method.

[0145] Specifically, it is preferably used in a method for manufacturing a semiconductor device and a method for cleaning a semiconductor manufacturing device. More specifically, the chemical liquid is preferably used for a purpose selected from the group consisting of a developer, a rinse liquid, a pre-wet liquid, a resist cleaning liquid, and a pipe cleaning liquid. In addition, the chemical liquid can also be used as an edge rinse liquid, a back rinse liquid, and a diluent for dilution.

[0146] The developer is used to remove the exposed part or the unexposed part from the resist film after exposure, and is used to form a resist pattern. As the organic solvent contained in the developer, it is preferably a mixed solvent comprising butyl acetate (nBA), 4-methyl-2-pentanol (methyl isobutyl carbinol, MIBC), propylene glycol monomethyl ether acetate (PGMEA) or propylene glycol monomethyl ether acetate (PGMEA) and one or more liquid organic acids selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid and lactic acid. In the case where the resist film is a metal resist, it is preferably used to include a developer comprising a mixed solvent, the mixed solvent comprising propylene glycol monomethyl ether acetate (PGMEA) and one or more liquid organic acids selected from the group consisting of formic acid, acetic acid, propionic acid, butyric acid and lactic acid.

[0147] The rinse solution is mainly used to clean the resist film after the above development.

[0148] The edge rinse liquid is a rinse liquid supplied to the periphery of the semiconductor substrate to remove the resist film at the periphery of the semiconductor substrate. The organic solvent contained in the rinse liquid is preferably butyl acetate (nBA), isopropyl alcohol (IPA) or 4-methyl-2-pentanol (MIBC).

[0149] The pre-wetting liquid is supplied to the semiconductor substrate before the resist film is formed, and is used to make the resist liquid easy to spread on the semiconductor substrate and form a uniform resist film with a smaller amount of resist liquid supplied. As the organic solvent contained in the pre-wetting liquid, cyclohexanone (CHN), propylene glycol monomethyl ether acetate (PGMEA) or isopropyl alcohol (IPA) is preferred.

[0150] The resist cleaning liquid is used for cleaning a semiconductor substrate on which a resist pattern is formed (stripping of the resist pattern). As the organic solvent contained in the resist cleaning liquid, propylene glycol monomethyl ether acetate (PGMEA) is preferred.

[0151] The pipe cleaning liquid is used, for example, for cleaning the pipes of semiconductor manufacturing equipment. The organic solvent contained in the pipe cleaning liquid is preferably propylene glycol monomethyl ether acetate (PGMEA), cyclohexanone (CHN), butyl acetate (nBA), isopropyl alcohol (IPA) or 4-methyl-2-pentanol (MIBC).

[0152] As the resist composition for forming the resist film, a known resist composition can be used.

[0153] Furthermore, the resist composition may be a so-called metal resist composition.

[0154] Examples of the metal resist composition include a photosensitive composition capable of forming a coating layer including a metal oxo-hydroxy network having an organic ligand via a metal-carbon bond and / or a metal carboxylate bond.

[0155] Examples of the metal resist composition include compositions described in Japanese Patent Application Laid-Open No. 2019-113855, and the contents are incorporated into the specification of the present application.

[0156] In addition, the organic solvent contained in the developer, rinser and resist cleaning solution is preferably acetic acid, butyl acetate, 4-methyl-2-pentanol, propionic acid, butyric acid, butyl butyrate, isobutyl isobutyrate, formic acid, isoamyl formate, isoamyl ether, amyl propionate, isoamyl propionate, ethylcyclohexane, mesitylene, decane, undecane, 3,7-dimethyl-3-octanol, 2-ethyl-1-hexanol, 1-octanol, 2-octanol, ethyl acetoacetate, dimethyl malonate, methyl pyruvate, dimethyl oxalate, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monomethyl ether (PGME), methyl ethyl ketone (MEK), 2-pentanol and isopropyl alcohol (IPA) and other organic solvents. In addition, it can also be a mixed solvent in which two or more organic solvents selected from the group consisting of the above-mentioned organic solvents are mixed in an arbitrary ratio.

[0157] As described above, the chemical solution of the present invention contains an organic solvent and metal-containing particles, wherein the metal-containing particles contain a metal element selected from the group consisting of Fe, Ni and Zn, wherein the I value of the chemical solution obtained by the above method X is 0.010 to 10.000.

[0158] In the case of the process for contacting the liquid medicine of the present invention with the contacted object, the mechanism by which the contacted object is not prone to defects may not be clear, but the inventors speculate as follows. In addition, the following mechanism is a speculation, and even if the subject of the present invention is solved by a mechanism other than the following mechanism, it is also included in the scope of the present invention.

[0159] The inventors of the present invention have been conducting in-depth research on the causes of defects when a chemical solution is applied to a process of contacting the chemical solution with various contact objects. As a result, it was found for the first time that when the above-mentioned I value is 10.000 or less, defects (particle defects) caused by the above-mentioned metal-containing particles are not easily generated. Furthermore, when the above-mentioned I value is 0.010 or more, since a certain amount of the above-mentioned metal-containing particles is contained, it is believed that the charging of the chemical solution can be alleviated, and problems corresponding to various uses can be suppressed in each non-contact object through the mechanism described below.

[0160] In the case where the contacted object is a resist film or resist pattern after exposure, the purpose of the liquid is a developer or a rinse solution. When the above-mentioned I value is 0.010 or more, by easing the charging of the liquid, the repulsive force or attractive force generated by the charging of the liquid is not easy to act on the resist pattern, and as a result, defects (pattern collapse) can be suppressed. In addition, there is a tendency that the above-mentioned defects (pattern collapse) are more likely to occur when the line width of the resist pattern is small.

[0161] In addition, when the contacted object is a semiconductor substrate (such as a silicon wafer), the purpose of the liquid medicine is a pre-wetting liquid. When the above-mentioned I value is more than 0.010, by relaxing the charging of the liquid medicine, the charging of the contacted semiconductor substrate surface is relaxed, and the composition used for the formation of the resist film applied in the subsequent process is easily and evenly wetted and spread. As a result, it is not easy to produce defects (uneven coating of the resist). Even if the above-mentioned non-contact object has a resist lower film on the semiconductor substrate, it is also believed that the effect can be obtained by the same mechanism.

[0162] In addition, when the contacted object has a semiconductor substrate (e.g., a silicon wafer) and one or more selected from the group consisting of a resist film and a resist pattern (hereinafter, also referred to as "resist film, etc."), the use of the liquid is a resist cleaning liquid. When the above-mentioned I value is 0.010 or more, by easing the charging of the liquid, the charging of the semiconductor substrate surface and the resist film, etc., which are contacted, is eased, and it is easy to wet and spread on the surface of the semiconductor substrate surface and the resist film, etc. As a result, the resist cleaning liquid easily contacts the entire surface of the resist film, etc., and the resist film, etc. is easily peeled off, and defects (generation of resist residues) are not easy to occur.

[0163] In addition, when the contacted object is a pipe (e.g., a pipe of a semiconductor manufacturing device), the purpose of the liquid medicine is a pipe cleaning liquid. When the above-mentioned I value is 0.010 or more, by relieving the charging of the liquid medicine, it is not easy to generate charging between the pipe wall and the liquid medicine when the liquid medicine is passed into the pipe, and it is not easy to generate sparks. As a result, particle defects in the process after the pipe cleaning can be suppressed.

[0164] Therefore, it is believed that in the process of bringing the liquid medicine of the present invention into contact with the object to be contacted, the object to be contacted is less likely to have defects, and the occurrence of problems corresponding to various uses can be suppressed. It is believed that in the objects to be contacted and uses other than the above, the object to be contacted is less likely to have defects through the same or similar mechanism.

[0165] Furthermore, Fe, Ni and Zn are often contained in larger amounts in organic solvents than other metal elements, and particles containing these elements are likely to remain even after filtration, and are considered to be metal-containing particles that dominate the properties of the chemical solution containing the organic solvent.

[0166] When the chemical solution is used as a developer or rinser, the I value is preferably 0.010 to 5.000, more preferably 0.010 to 1.200.

[0167] When the chemical solution is used as a pre-wetting solution, the I value is preferably 0.010 to 5.000, and more preferably 0.030 to 2.200.

[0168] When the chemical solution is used as a resist cleaning solution, the I value is preferably 0.010 to 5.000, and more preferably 0.020 to 2.400.

[0169] When the chemical liquid is used as a pipe cleaning liquid, the I value is preferably 0.010 to 5.000, and more preferably 0.020 to 2.400.

[0170] <Method for producing liquid medicine>

[0171] There is no particular limitation on the method for producing the above-mentioned drug solution, and a known method can be used. Among them, from the perspective of being able to more easily obtain the above-mentioned drug solution, a method for producing the drug solution having the following steps in sequence is preferred. Each step is described in detail below.

[0172] (1) Organic solvent preparation step of preparing an organic solvent

[0173] (2) Filtration step of passing the purified product containing an organic solvent through a filter to obtain a drug solution

[0174] [(1) Organic solvent preparation step of preparing an organic solvent]

[0175] The organic solvent preparation step is a step for preparing an organic solvent. There are no particular restrictions on the method for preparing an organic solvent, and for example, methods such as preparing by purchasing an organic solvent, and obtaining an organic solvent as a reactant by reacting raw materials can be cited. In addition, as an organic solvent, it is preferred to prepare an organic solvent containing metal particles and / or organic impurities containing a metal element (for example, the content of the organic solvent is 99% by mass or more). As a commercially available product of such an organic solvent, for example, a commercially available product called a "high-purity grade product" can be cited.

[0176] Furthermore, the prepared organic solvent may be composed of a single compound or may be a mixed organic solvent composed of a mixture of two or more compounds.

[0177] The method of obtaining an organic solvent as a reactant by reacting raw materials is not particularly limited, and a known method can be used. For example, there can be mentioned a method of obtaining an organic solvent by reacting one or more raw materials in the presence of a catalyst.

[0178] More specifically, for example, there can be mentioned: a method for obtaining butyl acetate by reacting acetic acid and n-butanol in the presence of sulfuric acid; a method for obtaining 1-hexanol by reacting ethylene, oxygen and water in the presence of Al(C2H5)3; a method for obtaining 4-methyl-2-pentanol by reacting cis-4-methyl-2-pentene in the presence of Ipc2BH (Diisopinocampheylborane); a method for obtaining PGMEA (propylene glycol 1-monomethyl ether 2-acetate) by reacting propylene oxide, methanol and acetic acid in the presence of sulfuric acid; a method for obtaining IPA (isopropyl alcohol) by reacting acetone and hydrogen in the presence of copper oxide-zinc oxide-aluminum oxide; a method for obtaining ethyl lactate by reacting lactic acid and ethanol; and the like.

[0179] [(2) Filtration step of passing the product to be purified containing an organic solvent through a filter to obtain a drug solution]

[0180] The filtration step is a step of passing the substance to be purified containing the organic solvent through a filter to obtain a drug solution. In this specification, the substance to be purified refers to, for example, the reaction product obtained in the organic solvent preparation step, the purified product obtained in the distillation step described later, and the organic solvent prepared by purchasing in the organic solvent preparation step.

[0181] From the viewpoint of facilitating the manufacture of the liquid medicine of the present invention, as a specific step of the filtration process, it is preferred that the purified product containing the organic solvent is filtered by sequentially passing through a first metal ion adsorption filter, a first particle removal filter having a pore size of 10 nm or less, a second metal ion adsorption filter, a second particle removal filter having a pore size of 10 nm or less, a third metal ion adsorption filter, and a third particle removal filter having a pore size of 10 nm or less. In addition, the first particle removal filter, the second particle removal filter, and the third particle removal filter are respectively made of different materials, and are respectively selected from the group consisting of fluororesins, polyamide-based resins, and polyolefin-based resins.

[0182] In the filtration step, the filtration treatment from the first metal ion adsorption filter to the third particle removal filter may be repeated. The number of cycles is, for example, preferably 2 to 8 times, more preferably 2 to 5 times.

[0183] The above method can effectively reduce the I value and adjust the I value to the range of the present invention. The detailed mechanism by which the I value can be adjusted to the range of the present invention by the above method is not necessarily clear, but is presumed as follows.

[0184] It can be considered that the chemical properties of Fe, Ni and Zn are different, and there are differences in the behavior of particles containing Fe, particles containing Ni and particles containing Zn in organic solvents. For example, if the elements contained in the particles are different, the surface potential of the particles in the organic solvent is different in most cases. If the surface potential of the particles is different, it can be said that the interaction with other objects such as particle removal filters in the organic solvent is different. Therefore, in a single particle removal filter, it is possible to become a state where the removal rate of particles containing specific elements is low. Therefore, it can be considered that as in the above method, using a first particle removal filter, a second particle removal filter and a third particle removal filter with different materials, all types of particles containing Fe, particles containing Ni and particles containing Zn can be effectively removed, and as a result, the I value can be effectively reduced.

[0185] In addition, it can be considered that Fe, Ni and Zn can also exist as ions in the organic solvent, and can be considered to be in a state of equilibrium between the form of particles and the form of ions. Here, it can be said that even if the particles are removed by the particle removal filter, the ions cannot be removed by the particle removal filter. If the ions are not removed, particles may be generated from the remaining ions. On the contrary, it can be said that even if only ions are removed by the ion removal filter, ions may be generated from the remaining particles. Here, it can be considered that when the organic solvent is alternately passed through the ion removal filter and the particle removal filter, both particles and ions can be removed before the other is generated by either party, and as a result, the I value can be effectively reduced.

[0186] On the other hand, in the particle removal filter, it is not easy to supplement particles smaller than the filter aperture, and it can be said that there is a deviation in the filter aperture, so it is difficult to completely remove the particles. In addition, it is difficult to remove particles in the ion removal filter. Therefore, if the number of cycles is appropriately set, the I value can be adjusted to the scope of the present invention.

[0187] The above-mentioned filtration step will be described in detail below.

[0188] (Metal ion adsorption filter)

[0189] In the above-mentioned filtration step, the first to third metal ion adsorption filters are used. By using these filters, the ions in the object to be purified can be reduced.

[0190] The first to third metal ion adsorption filters may be filters of the same type or filters of different types.

[0191] The metal ion adsorption filter is not particularly limited, and a known metal ion adsorption filter may be used.

[0192] Among them, as the metal ion adsorption filter, a filter capable of ion exchange is preferred. Here, the metal ion to be adsorbed is preferably an ion of at least one metal selected from the group consisting of Fe, Ni and Zn, and more preferably an ion of all metals of Fe, Ni and Zn.

[0193] From the viewpoint of improving the metal ion adsorption performance, the metal ion adsorption filter preferably has an acid group on the surface. Examples of the acid group include a sulfonic group and a carboxyl group.

[0194] Examples of the base material (material) constituting the metal ion adsorption filter include cellulose, diatomaceous earth, nylon, polyethylene, polypropylene, polystyrene, and fluororesin.

[0195] In addition, the metal ion adsorption filter may be composed of a material containing polyimide and / or polyamide-imide. As the metal ion adsorption filter, for example, a polyimide and / or polyamide-imide porous membrane described in Japanese Patent Application Laid-Open No. 2016-155121 can be cited.

[0196] The polyimide and / or polyamideimide porous membrane may contain at least one selected from the group consisting of a carboxyl group, a salt-type carboxyl group, and an -NH- bond. If the metal ion adsorption filter is made of fluororesin, polyimide and / or polyamideimide, it has better solvent resistance.

[0197] There are no particular limitations on the method for passing the object to be purified through the metal ion adsorption filters (the first metal ion adsorption filter to the third metal ion adsorption filter), and examples thereof include: disposing a metal ion adsorption filter unit having a metal ion adsorption filter and a filter housing in the middle of a transfer pipeline for transferring the object to be purified, and passing the object to be purified through the metal ion adsorption filter unit under pressure or without pressure.

[0198] (Particle Removal Filter)

[0199] In the above-mentioned filtering step, the first to third particle removal filters are used. By using these filters, the particle components containing a predetermined metal element in the object to be purified can be reduced.

[0200] The first to third particle removal filters are different types of filters, that is, the first to third particle removal filters are made of different materials, respectively, and are selected from the group consisting of fluororesins, polyamide resins, and polyolefin resins.

[0201] Furthermore, for example, when the first particle removal filter is made of polypropylene and the second particle removal filter is made of polyethylene, the two correspond to a mode in which the materials are different.

[0202] The pore diameter (particle removal diameter) of the first to third particle removal filters is 10 nm or less, preferably 8 nm or less, and more preferably 5 nm or less. The lower limit is not particularly limited, but is often 1 nm or more.

[0203] Here, the pore size (particle removal size) refers to the minimum size of particles that can be removed by the filter. For example, when the particle removal size of the filter is 10 nm, particles with a diameter of 10 nm or more can be removed.

[0204] The material of the first to third particle removal filters is selected from the group consisting of fluororesins, polyamide resins, and polyolefin resins, and examples thereof include 6-nylon, 6,6-nylon, polyethylene, polypropylene, and polytetrafluoroethylene (PTFE).

[0205] The polyimide-based resin may have at least one selected from the group consisting of a carboxyl group, a salt-type carboxyl group, and a -NH- bond.

[0206] There is no particular limitation on the method for passing the object to be purified through the particle removal filters (first particle removal filter to third particle removal filter), and the following method can be cited: a particle removal filter unit having a particle removal filter and a filter housing is arranged in the middle of a transfer pipeline for transferring the object to be purified, and the object to be purified is passed through the above-mentioned particle removal filter unit under pressure or without pressure.

[0207] In the filtration step, the temperature of the product to be purified when the product to be purified passes through the filter is not particularly limited, but is generally preferably 0 to 30°C, more preferably 0 to 15°C.

[0208] Since the filtration pressure affects the filtration accuracy, it is preferable to reduce the pulsation of the pressure during filtration as much as possible.

[0209] In the above-mentioned method for producing a drug solution, the filtration rate is not particularly limited, but is preferably 1.0 L / min / m 2 More preferably, 0.75 L / min / m 2 More preferably, 0.6 L / min / m 2 above.

[0210] The filter is set with a pressure differential that guarantees filter performance (does not damage the filter). When this value is large, the filtration speed can be increased by increasing the filtration pressure. That is, the upper limit of the filtration speed usually depends on the pressure differential of the filter, and is usually preferably 10.0 L / min / m 2 the following.

[0211] In the above-mentioned method for producing a drug solution, the filtration pressure is preferably 0.001 to 1.0 MPa, more preferably 0.003 to 0.5 MPa, and even more preferably 0.005 to 0.3 MPa. In particular, when using a filter with a small pore size, by increasing the filtration pressure, the amount of particulate foreign matter or impurities dissolved in the purified product can be effectively reduced. When using a filter with a pore size of less than 20 nm, the filtration pressure is particularly preferably 0.005 to 0.3 MPa.

[0212] As long as the filtration step includes a process of passing the object to be purified through the first metal ion adsorption filter to the third particle removal filter, another filter may be further provided to allow the object to be purified to pass therethrough.

[0213] [(3) Optional process]

[0214] The method for producing the above-mentioned chemical solution may include an organic impurity removal step, a distillation step, a water content adjustment step, and a static elimination step as optional steps other than the above-mentioned filtration step. Each of the above-mentioned optional steps will be described in detail below.

[0215] (Organic impurity removal process)

[0216] The filtration step may further include an organic impurity removal step. As the organic impurity removal step, it is preferably a step of passing the purified product through an organic impurity adsorption filter. There is no particular limitation on the method of passing the purified product through the organic impurity adsorption filter, and the following method may be mentioned: a filtration unit including an organic impurity adsorption filter and a filter housing is arranged in the middle of a transfer line for transferring the purified product, and an organic solvent is passed through the filtration unit under pressure or without pressure.

[0217] The organic impurity adsorption filter is not particularly limited, and a known organic impurity adsorption filter may be used.

[0218] Among them, as an organic impurity adsorption filter, from the viewpoint of improving the adsorption performance of organic impurities, it is preferred to have an organic skeleton that can interact with organic impurities on the surface (in other words, the surface is modified by an organic skeleton that can interact with organic impurities). As an organic skeleton that can interact with organic impurities, for example, a chemical structure that can react with organic impurities and capture organic impurities into an organic impurity adsorption filter can be cited. More specifically, in the case where n-long-chain alkyl alcohol (structural isomer when 1-long-chain alkyl alcohol is used as an organic solvent) is included as an organic impurity, an alkyl group can be cited as an organic skeleton. In addition, in the case where butylated hydroxytoluene (BHT) is included as an organic impurity, a phenyl group can be cited as an organic skeleton.

[0219] Examples of the substrate (material) constituting the organic impurity adsorption filter include cellulose, diatomaceous earth, nylon, polyethylene, polypropylene, polystyrene, and fluororesin on which activated carbon is supported.

[0220] In addition, as the organic impurity adsorption filter, a filter in which activated carbon is fixed to a nonwoven fabric as described in Japanese Patent Application Laid-Open Nos. 2002-273123 and 2013-150979 may be used.

[0221] As the organic impurity adsorption filter, in addition to the chemical adsorption (adsorption using an organic impurity removal filter having an organic skeleton on the surface that can interact with organic impurities) described above, a physical adsorption method can also be applied.

[0222] For example, in the case where BHT is contained as an organic impurity, the structure of BHT is larger than Therefore, by using an organic impurity adsorption filter with a pore size of 1 nm, BHT cannot pass through the pores of the filter. That is, BHT is physically captured by the filter and can be removed from the purified product. In this way, not only chemical interactions but also physical removal methods can be applied to the removal of organic impurities. However, in this case, a filter with a pore size of 3 nm or more is used as a "particle removal filter", and a filter with a pore size of less than 3 nm is used as an "organic impurity adsorption filter".

[0223] In this manual, (Angstrom) is equivalent to 0.1nm.

[0224] (Distillation process)

[0225] The method for producing the above-mentioned drug solution may include a distillation step. The distillation step refers to a step of distilling an organic solvent or a reactant to obtain a purified product. There is no particular limitation on the distillation method, and a known method can be used.

[0226] When the method for producing the above-mentioned drug solution includes a distillation step, the order of the steps described above is not particularly limited. From the viewpoint of more easily obtaining the above-mentioned drug solution, it is preferred to include the distillation step after the organic solvent preparation step and before the filtration step.

[0227] (Water content adjustment process)

[0228] The method for producing the above-mentioned liquid medicine may include a water content adjustment step. The water content adjustment step is a step for adjusting the water content contained in the purified product. There is no particular limitation on the method for adjusting the water content, and examples thereof include a method of adding water to the purified product and a method of removing water from the purified product.

[0229] The method for removing water is not particularly limited, and a known dehydration method can be used.

[0230] Examples of the method for removing water include a dehydration membrane, a water adsorbent insoluble in an organic solvent, an aeration replacement device using a dry inert gas, and a heating or vacuum heating device.

[0231] When a dehydration membrane is used, membrane dehydration is performed by pervaporation (PV) or vapor permeation (VP). The dehydration membrane is, for example, constructed in the form of a water-permeable membrane module. As the dehydration membrane, a membrane made of a polymer such as polyimide, cellulose, and polyvinyl alcohol, or an inorganic material such as zeolite can be used.

[0232] A water adsorbent may be added to the product to be purified. Examples of the water adsorbent include zeolite, phosphorus pentoxide, silica gel, calcium chloride, sodium sulfate, magnesium sulfate, anhydrous zinc chloride, fuming sulfuric acid, and soda lime.

[0233] In addition, when zeolite (particularly, Molecular Sieve (trade name) manufactured by UNION Showa Co., Ltd., etc.) is used in the dehydration treatment, olefins can also be removed.

[0234] (Electrical removal process)

[0235] The method for producing the chemical solution may include a static elimination step. The static elimination step is a step of reducing the charge potential of the object to be purified by static elimination of the object to be purified.

[0236] There are no particular limitations on the method for removing static electricity, and a known method for removing static electricity can be used. For example, the method of bringing the object to be purified into contact with a conductive material can be cited.

[0237] The contact time of the purified object and the conductive material is preferably 0.001 to 60 seconds, more preferably 0.001 to 1 second, and even more preferably 0.01 to 0.1 second. Examples of the conductive material include stainless steel, gold, platinum, diamond, and glassy carbon.

[0238] Examples of a method for bringing the object to be purified into contact with the conductive material include a method in which a grounded mesh made of a conductive material is disposed inside a pipeline and the object to be purified is passed therethrough.

[0239] It is preferable that the static elimination step is performed before at least one step selected from the group consisting of an organic solvent preparation step, a distillation step, and a filtration step.

[0240] In addition, each of the steps described above is preferably performed in a sealed state and under an inert gas atmosphere in which the possibility of water mixing into the product to be purified is low.

[0241] In order to minimize the incorporation of water, each step is preferably performed in an inert gas atmosphere having a dew point temperature of -70°C or lower. This is because the water concentration in the gas phase is 2 mass ppm or lower in an inert gas atmosphere at -70°C or lower, so the possibility of water incorporation into the purified product is reduced.

[0242] Furthermore, in addition to the above-mentioned steps, the method for producing a chemical solution may include, for example, an adsorption purification treatment step of a metal component using silicon carbide as described in International Publication No. WO2012 / 043496.

[0243] In the method for manufacturing the above-mentioned liquid medicine, it is preferred that the portion in contact with the liquid medicine in the device related to the manufacturing be cleaned before the liquid medicine of the present invention is manufactured. The liquid used in the cleaning is not particularly limited, but is preferably the liquid medicine itself or a diluent after diluting the liquid medicine. Alternatively, an organic solvent that substantially does not contain or sufficiently reduces particles containing metal atoms, metal ion components and organic impurities can be used. Cleaning can be performed multiple times, and two or more organic solvents can be used, or they can be mixed and used. It can be a cyclic cleaning. Whether the device related to the manufacturing has been sufficiently cleaned can be judged by measuring the content of particles containing metal atoms, metal ion components and organic impurities contained in the liquid used for cleaning.

[0244] <Container>

[0245] The above-mentioned drug solution can be temporarily stored in a container until use. There is no particular limitation on the container for storing the above-mentioned drug solution, and a known container can be used.

[0246] As a container for storing the chemical solution, it is preferable to use a container for semiconductor use, which has high cleanliness inside the container and little elution of impurities.

[0247] Specific examples of usable containers include the "Clean Bottle" series manufactured by AICELLO Chemical Co., Ltd. and the "Pure Bottle" manufactured by Kodama Resin Industries, but the containers are not limited thereto.

[0248] The liquid contact portion of the container is preferably formed of a non-metallic material.

[0249] Examples of the non-metallic material include the materials exemplified in the non-metallic material used for the liquid contact portion of the above-mentioned distillation column.

[0250] In particular, among the above, when a container whose liquid contact portion is made of fluororesin is used, the occurrence of the disadvantage of elution of ethylene or propylene oligomers can be suppressed compared to the case of using a container whose liquid contact portion is made of polyethylene resin, polypropylene resin or polyethylene-polypropylene resin.

[0251] As a specific example of such a container whose liquid contact part is a fluororesin, for example, a FluoroPure PFA composite drum manufactured by Entegris can be cited. In addition, containers described in page 4 of Japanese Patent Publication No. 3-502677, page 3 of International Publication No. 2004 / 016526, and pages 9 and 16 of International Publication No. 99 / 46309 can also be used. In addition, when the liquid contact part is made of a non-metallic material, it is preferred to suppress the dissolution of the non-metallic material into the liquid medicine.

[0252] It is also preferred that the container has a liquid contact portion that contacts the chemical solution made of a metal material containing Cr atoms and Fe atoms, and the metal material is at least one selected from the group consisting of stainless steel and electrolytically polished stainless steel.

[0253] The above-mentioned stainless steel has been described as the material of the liquid contact part of the distillation tower, and the same applies to the electrolytically ground stainless steel.

[0254] The container is preferably cleaned before containing the solution. The liquid used for cleaning is preferably the above-mentioned liquid medicine itself or a diluent obtained by diluting the above-mentioned liquid medicine. The above-mentioned liquid medicine can be bottled in a container such as a gallon bottle or a coated bottle after production for transportation and storage. The gallon bottle can be a bottle made of glass material or a bottle made of other materials.

[0255] In order to prevent the composition of the solution from changing during storage, the container may be replaced with an inert gas (nitrogen or argon, etc.) with a purity of 99.99995% by volume or more. A gas with a low water content is particularly preferred. In addition, during transportation and storage, the temperature may be room temperature, but in order to prevent deterioration, the temperature may also be controlled in the range of -20°C to 30°C.

[0256] It is preferred that the operations including the manufacture of the above-mentioned drug solution, opening and / or cleaning of the container, and storage of the solution, processing analysis, and measurement are all performed in a clean room. The clean room preferably meets the 14644-1 clean room standard. It is preferred to meet any one of ISO (International Organization for Standardization) level 1, ISO level 2, ISO level 3, and ISO level 4, more preferably ISO level 1 or ISO level 2, and even more preferably ISO level 1.

[0257] <Drug Solution Container>

[0258] The drug solution of the present invention may be in the form of a drug solution container including a container and the drug solution contained in the container.

[0259] It is also preferable that the liquid contact portion in the container that contacts the chemical solution is formed of a metal material containing Cr atoms and Fe atoms, and the metal material is at least one selected from the group consisting of stainless steel and electrolytically polished stainless steel.

[0260] In addition, the form of the above-mentioned container has been described as a preferred form of a container capable of containing a medical solution.

[0261] <Method for Manufacturing Drug Solution Container>

[0262] There is no particular limitation on the method for manufacturing the above-mentioned drug solution container, and a known manufacturing method can be used. Among them, from the perspective of being able to more easily obtain the above-mentioned drug solution container, a method for manufacturing a drug solution having the following steps in sequence is preferred. Each step is described in detail below.

[0263] (1) Organic solvent preparation step of preparing an organic solvent

[0264] (2) Filtration step of passing the purified product containing an organic solvent through a filter to obtain a drug solution

[0265] (3) A step of storing the drug solution in a container to obtain a drug solution container

[0266] [(1) Organic solvent preparation step of preparing an organic solvent]

[0267] The method for producing the drug solution container preferably includes an organic solvent preparation step. The organic solvent preparation step is as described above as the method for producing the drug solution.

[0268] [(2) Filtration step of passing the product to be purified containing an organic solvent through a filter to obtain a drug solution]

[0269] The method for producing the drug solution container preferably includes a filtration step. The filtration step is as described above as the method for producing the drug solution.

[0270] [(3) Step of accommodating the drug solution in a container to obtain a drug solution container]

[0271] The method for producing the drug solution container preferably includes a containing step. There is no particular limitation on the method for containing the drug solution in the container, and a known containing method can be used.

[0272] In addition, the form of the container is as described above as the form of the container provided in the drug solution container.

[0273] In the containing step, the temperature of the drug solution when containing the drug solution in the container is not particularly limited, but is generally preferably 0 to 30°C, and more preferably 0 to 10°C.

[0274] As a method for containing a drug solution in a container, it is more preferable to contain the drug solution in a container using the following containing device from the viewpoint of being able to more easily obtain the above-mentioned drug solution container and making it more difficult for undesired impurities to be mixed into the drug solution during the drug solution containing step.

[0275] (Containment device)

[0276] As one form of a container device that can be used in the above-mentioned drug solution containing process, the following container device can be cited: it is a container device having a drug solution containing portion, and the liquid contact portion of the drug solution containing portion is formed by at least one selected from the group consisting of non-metallic materials and electrolytically polished metal materials.

[0277] The forms of the non-metallic material and the electrolytically ground metal material are as described above as the material of the liquid contact part of the distillation apparatus.

[0278] (Container (Other Forms))

[0279] As other forms of a container device that can be used in the above-mentioned drug solution containing process, the following container device can be cited: the container device is provided with a drug solution containing portion and a drug solution supply pipeline connected to the drug solution containing portion and used to supply the drug solution to the drug solution supply portion, wherein the liquid contact portion of the drug solution supply pipeline is formed by at least one selected from the group consisting of non-metallic materials and electrolytically ground metal materials.

[0280] The forms of the non-metallic material and the electrolytically ground metal material are as described above as the material of the liquid contact part of the distillation apparatus.

[0281] The container device involved in this form is equipped with a liquid medicine supply pipeline connected to the liquid medicine container. The liquid medicine supply pipeline is connected to the pipeline used in the filtration process to transfer the purified material. Therefore, the liquid medicine obtained by the filtration process is moved to the liquid medicine container in a closed system, which can further suppress the mixing of impurities into the liquid medicine.

[0282] <Preferred Embodiment of the Method for Manufacturing the Drug Solution Container>

[0283] As a method for producing the above-mentioned drug solution container, it is more preferable to have the following steps.

[0284] (1) Organic solvent preparation step of preparing an organic solvent

[0285] (2) Filtration step of passing the purified product containing an organic solvent through a filter to obtain a drug solution

[0286] (3) A step of storing the drug solution in a container to obtain a drug solution container

[0287] The organic solvent preparation step and the filtration step are as described above as the method for producing the drug solution. The storage step is as described above as the method for producing the drug solution container.

[0288] According to the method for manufacturing the drug solution container, the drug solution container can be manufactured more simply.

[0289] <Method for producing resist pattern>

[0290] The above-mentioned chemical solution can be used in a method for producing a resist pattern.

[0291] It is preferred that a general method for producing a resist pattern includes the following steps, and the above-mentioned chemical solution is used in any of the steps of the following production method.

[0292] Step 1: Step of forming a resist film on a semiconductor substrate using a resist composition

[0293] Step 2: Step of exposing the resist film to a pattern

[0294] Step 3: A step of developing the resist film after pattern exposure using a developer to obtain a resist pattern

[0295] Furthermore, before step 1, step 4 of applying a pre-wetting liquid on the substrate may be included.

[0296] In addition, after the step 3, a step 5 of rinsing the resist pattern using a rinsing liquid may be included.

[0297] Furthermore, after step 3 or after step 5, step 6 of stripping the resist pattern using a resist cleaning solution may be included.

[0298] The above-mentioned chemical solution can be used as an organic solvent contained in, for example, a pre-wetting solution, a developing solution, a rinsing solution, a resist cleaning solution, and the like.

[0299] In step 1, a known resist composition can be used as the resist composition.

[0300] The resist composition can be applied by a known coating method and coating apparatus (for example, a coating and developing device).

[0301] In addition, as the semiconductor substrate, a known semiconductor substrate (silicon wafer, etc.) can be used.

[0302] In step 2, a known method can be used for the exposure method of the resist film. Examples of the light source used for exposure include extreme ultraviolet rays, X-rays, EUV, and particle beams such as electron beams and ion beams.

[0303] In step 3, a known method can be used as the developing method.

[0304] The chemical solution can also be applied to a method for manufacturing a semiconductor device having a process using the chemical solution. Examples of the process using the chemical solution include the processes of the method for manufacturing a resist pattern, cleaning of a semiconductor substrate using the chemical solution, and cleaning of a semiconductor manufacturing device using the chemical solution (e.g., cleaning of piping).

[0305] [Example]

[0306] Hereinafter, the present invention will be described in more detail based on examples.

[0307] The materials, amounts, ratios, treatment contents and treatment procedures shown in the following examples may be appropriately changed without departing from the gist of the present invention. Therefore, the scope of the present invention should not be interpreted in a restrictive manner by the following examples.

[0308] In addition, when preparing the drug solutions of the examples and comparative examples, the operation of the containers, the preparation, filling, storage and analysis of the drug solutions were all carried out in a clean room that meets the ISO Class 2 or 1 level.

[0309] <Manufacturing of liquid medicine>

[0310] The product to be purified including the organic solvent was purified under the conditions shown in the table below to obtain the chemical solution used in each of the Examples and Comparative Examples.

[0311] In addition, for each chemical solution, the purified product was passed through each filter (first filter to sixth filter) listed in the table, and the passage through each filter was repeated the number of times indicated in the "Number of cycles" column. In addition, chemical solutions with blank columns in the filter column indicate that the filter was not used.

[0312] In addition, for example, the expression "PGMEA80 / acetic acid 20" in the table means that a solvent obtained by mixing 80 mass % of PGMEA and 20 mass % of acetic acid is used as the product to be purified.

[0313] In addition, the purified products listed in the table were prepared in different batches, and therefore the components other than the organic solvent initially contained in each purified product may be different.

[0314] In addition, in the table, racemic lactic acid was used for "lactic acid".

[0315] The abbreviations in the table are explained below.

[0316] [Organic solvents]

[0317] nBA: Butyl acetate

[0318] MIBC: 4-methyl-2-pentanol

[0319] ·CHN:Cyclohexanone

[0320] ·PGMEA: Propylene glycol monomethyl ether acetate

[0321] IPA: Isopropyl alcohol

[0322] [Filter]

[0323] IEX: Ion exchange filter ("IonKlee" manufactured by Pall Corporation)

[0324] Nylon: Nylon filter ("Asymmetric" manufactured by Pall Corporation)

[0325] PP: Polypropylene filter (3M "NanoSHIELD")

[0326] PTFE: Polytetrafluoroethylene filter ("XpressKLEEN" manufactured by Pall Corporation)

[0327] UPE: Ultra-high molecular weight polyethylene filter ("Microgard" manufactured by Entegris)

[0328] In addition, when each filter has pores, the pore diameter is as described in the table.

[0329] <Measurement by LA-ICP-MS>

[0330] According to the above-described method X, samples using each drug solution were prepared and analyzed by LA-ICP-MS. The I value (counts / mm 2 ). In addition, the above-described method X is to analyze one element in one sample by LA-ICP-MS using a method using different samples to obtain each detection intensity map (C Fe , C Ni and C Zn The results are shown in the table below.

[0331] Furthermore, when the measurement was performed by the above method, Fe, Ni, and Zn were detected in each chemical solution.

[0332] <Evaluation of developer and rinser>

[0333] The occurrence of defects when using the chemical solution (Examples 1 to 20, Comparative Examples 1 to 20) as a developer or rinser was evaluated by the following method. In addition, the coating and developing equipment "RF 3S ”.

[0334] First, AL412 (manufactured by Brewer Science) was applied to a silicon wafer and baked at 200°C for 60 seconds to form a resist underlayer film with a thickness of 20 nm. A pre-wetting liquid (a mixed solvent of PGMEA and propylene carbonate in a ratio of 3:1) was applied thereon, and the resist composition 1 described later was further applied thereon. After the resist composition 1 was applied, baking (PB: Prebake) was performed at 100°C for 60 seconds to form a resist film with a thickness of 30 nm.

[0335] The resist film was exposed using an EUV exposure machine (manufactured by ASML; NXE3350, NA 0.33, dipole 90°, outer sigma 0.87, inner sigma 0.35) through a reflective mask having a pitch of 20 nm and a pattern width of 10 nm, and then heated at 85° C. for 60 seconds (PEB: Post Exposure Bake).

[0336] Next, in Examples 1 to 10 and Comparative Examples 1 to 10, the chemical solution of each Example and Comparative Example was used as a developer and development was performed for 30 seconds. Then, the wafer was rotated at 2000 rpm for 40 seconds to form a line and space pattern with a pitch of 20 nm and a pattern line width of 10 nm.

[0337] In Examples 11 to 20 and Comparative Examples 11 to 20, after PEB, the chemical solution of Example 1 was used as a developer for 30 seconds, and then rinsed with the chemical solution of each Example and Comparative Example for 20 seconds. Thereafter, patterns were formed in the same manner as in Examples 1 to 10 and Comparative Examples 1 to 10.

[0338] In the pattern formed by the above-mentioned steps, the number of occurrences of pattern collapse was measured using UVision8 manufactured by Applied Materials and SEMVision G7E, a fully automatic defect review and classification device manufactured by Applied Materials.

[0339] In addition, particle defects were measured using a combination of KLA-Tencor's SP-7 wafer inspection system and Applied Materials' SEMVision G7E fully automatic defect review and classification system.

[0340] In addition, particle defects refer to granular defects remaining in the formed pattern, and refer to defects whose particle diameter is 5nm or more. When measuring particle defects, the method described in paragraphs 0015 to 0067 of Japanese Patent Publication No. 2009-188333 was used for detection. That is, Si0 was formed on the wafer in advance by CVD (chemical vapor deposition) before the resist pattern was formed. xAfter forming a resist pattern, the resist was stripped by oxygen plasma, and the particles and Si0 x The etching is performed and the particles above the detection limit of the above-mentioned wafer inspection device are counted.

[0341] Hereinafter, the resist resin composition 1 used for the evaluation of the developer and the rinse solution will be described. The resist resin composition 1 is obtained by mixing the following components.

[0342] [Resist composition 1]

[0343] The resist composition 1 is obtained by mixing the components in the following composition.

[0344] Resin (A-1): 0.77 g

[0345] Acid generator (B-1): 0.03 g

[0346] Basic compound (E-3): 0.03 g

[0347] PGMEA: 67.5g

[0348] EL: 75g

[0349] (Resin (A), etc.)

[0350] (Synthesis Example 1) Synthesis of Resin (A-1)

[0351] 600 g of cyclohexanone was added to a 2L flask, and nitrogen substitution was performed at a flow rate of 100 mL / min for one hour. Then, 4.60 g (0.02 mol) of polymerization initiator V-601 (manufactured by Wako Pure Chemical Industries, Ltd.) was added, and the temperature was raised until the internal temperature reached 80°C. Next, the following monomers and 4.60 g (0.02 mol) of polymerization initiator V-601 (manufactured by Wako Pure Chemical Industries, Ltd.) were dissolved in 200 g of cyclohexanone to prepare a monomer solution. The monomer solution was added dropwise to the above-mentioned flask heated to 80°C over 6 hours. After the addition was completed, it was further reacted at 80°C for 2 hours.

[0352] 4-Acetoxystyrene 48.66 g (0.3 mol)

[0353] 1-Ethylcyclopentyl methacrylate 109.4 g (0.6 mol)

[0354] Monomer 122.2g (0.1mol)

[0355] [Chemical formula 1]

[0356]

[0357] The reaction solution was cooled to room temperature and added dropwise to 3 L of hexane to precipitate a polymer. The filtered solid was dissolved in 500 mL of acetone and added dropwise to 3 L of hexane again. The filtered solid was dried under reduced pressure to obtain 160 g of a 4-acetoxystyrene / 1-ethylcyclopentyl methacrylate / monomer 1 copolymer (A-1).

[0358] Add 10 g of the polymer obtained above, 40 mL of methanol, 200 mL of 1-methoxy-2-propanol and 1.5 mL of concentrated hydrochloric acid to a reaction container, heat to 80°C and stir for 5 hours. Cool the reaction solution to room temperature and add it dropwise to 3 L of distilled water. Dissolve the filtered solid in 200 mL of acetone, add it dropwise to 3 L of distilled water again, and dry the filtered solid under reduced pressure to obtain resin (A-1) (8.5 g). The weight average molecular weight (Mw) converted to standard polystyrene obtained by gel permeation chromatography (GPC) (solvent: THF (tetrahydrofuran)) is 11200, and the molecular weight dispersion (Mw / Mn) is 1.45. The composition is shown in Table 3 below.

[0359] [Table 1]

[0360]

[0361] (Photoacid generator (B))

[0362] As the photoacid generator, the following was used.

[0363] [Chemical formula 2]

[0364]

[0365] (Basic compound (E))

[0366] As the basic compound, the following were used.

[0367] [Chemical formula 3]

[0368]

[0369] In addition, the occurrence of defects when using chemical solutions (Examples 106 to 110, Comparative Examples 106 to 110) as rinse solutions was also evaluated by the same method as above. As a developer, butyl acetate (nBA) used in Example 1 was used.

[0370] <Evaluation of Metal Resist Developer>

[0371] The occurrence of defects when using chemical solutions (Examples 51 to 105, Comparative Examples 51 to 105) as metal resist developers was evaluated by the following method.

[0372] First, monobutyltin oxide hydrate (BuSnOOH) powder (0.209g, TCI America) was added to 4-methyl-2-pentanol (10mL) to prepare a metal resist precursor solution. The above solution was added to a closed medicine bottle and stirred for 24 hours. The resulting mixture was centrifuged at 4000rpm for 15 minutes, filtered by a 0.45μm PTFE (polytetrafluoroethylene) syringe filter, insoluble materials were removed, and metal resist composition R-1 was obtained.

[0373] In addition, the organic solvent in the metal resist composition R-1 is removed, the solid component is fired at 600 ° C, and the content of Sn is estimated according to the residual mass of SnO. As a result, the content of Sn in the metal resist composition R-1 is 0.093 mol / L. In addition, the dynamic light scattering (DLS) analysis of the metal resist precursor solution is performed using a Moebius device (Wyatt Technology). As a result, it is consistent with the unimodal distribution of particles with an average particle size of 2 nm, and is consistent with the diameter reported by the polyatomic cation of dodecamer butyltin hydroxide / oxide (Eychenne-Baron et al., Organometallics, 19, 1940-1949 (2000)).

[0374] Next, a base film forming composition SHB-A940 (manufactured by Shin-Etsu Chemical Co., Ltd.) was applied to a silicon wafer having a diameter of 300 mm, and baked at 205° C. for 60 seconds to form a base film having a film thickness of 20 nm. A metal resist composition R-1 was applied thereon so that the film thickness after drying reached 22 nm, and pre-baked at 100° C. for 90 seconds to form a metal resist film. Thus, a silicon wafer having a metal resist film was formed.

[0375] For the silicon wafer with the metal resist film, the EUV scanner NXE3400 (NA0.33, manufactured by ASML) was used to perform pattern exposure while changing the exposure amount. In addition, as the marking line, a hexagonal contact hole mask with a spacing of 36nm and an opening size of 21nm was used. After that, after 90 seconds of post-exposure baking (PEB) at 150°C, the solution of the embodiment and the comparative example was used as the developer, and the liquid was covered (pudd]e) for 30 seconds for negative development. After development, the wafer was rotated at a speed of 4000rpm for 30 seconds for drying, and a columnar pattern with a spacing of 36nm was obtained.

[0376] In the columnar pattern formed by the above-described steps, the number of particle defects and the number of pattern collapses were counted in the same manner as in the evaluation of the developer and rinser.

[0377] <Pre-wetting liquid evaluation>

[0378] The occurrence of defects when using the chemical solution (Examples 21 to 25 and 111 to 120, Comparative Examples 21 to 25 and 111 to 120) as the pre-wetting solution was evaluated by the following method. In addition, the coating and developing equipment "RF 3S ". In addition, the chemical solutions used in Examples 111 to 115 and Comparative Examples 111 to 115 were the same as the chemical solutions used in Examples 106 to 110 and Comparative Examples 106 to 110 for the evaluation of the rinsing solution. The chemical solutions used in Examples 116 to 120 and Comparative Examples 116 to 120 were the same as the chemical solutions used in Examples 16 to 20 and Comparative Examples 16 to 20 for the evaluation of the rinsing solution.

[0379] First, the same operation as the developer and rinse liquid evaluation was performed to form a resist lower layer film with a film thickness of 20nm. The above-mentioned coating and developing equipment was used thereon to apply the chemical solution of each embodiment as a pre-wetting liquid on the silicon wafer. After applying the chemical solution, the resist composition 1 used in the evaluation of the above-mentioned developer and rinse liquid was applied, and the uneven coating of the resist was observed and evaluated visually. The situation where obvious unevenness occurred visually was evaluated as B, and the situation where unevenness was not observed was evaluated as A.

[0380] In addition, the number of particle defects after the resist coating was counted in the same manner as in the evaluation of the developer and rinser.

[0381] <Evaluation of Resist Cleaning Liquid>

[0382] The occurrence of defects when using the chemical solutions (Examples 26 to 30, Comparative Examples 26 to 30) as resist cleaning solutions was evaluated by the following method.

[0383] In the same manner as the evaluation of the pre-wetting solution, a pre-wetting solution (a mixed solvent of PGMEA and propylene carbonate in a ratio of 3:1) was applied to a silicon wafer on which a resist underlayer film with a thickness of 20 nm was formed, and then the resist composition 1 used in the evaluation of the developer and rinse solution was applied to form a resist film. The formed resist film was 30 nm thick.

[0384] The formed resist film was supplied with a chemical solution as a resist cleaning solution and cleaned for 20 seconds. Then, the silicon wafer was rotated at 2000 rpm for 40 seconds to dry it.

[0385] The carbon content on the surface of the cleaned and dried silicon wafer was measured by X-ray photoelectron spectroscopy. The carbon content on the surface of the untreated silicon wafer was also measured in the same manner. The carbon content was measured at any 10 points on the silicon wafer, and the average value was taken as the carbon content.

[0386] The case where the carbon amount of the cleaned and dried silicon wafer was twice or more of the carbon amount of the unprocessed silicon wafer was evaluated as B, and the case where it was less than twice was evaluated as A.

[0387] In addition, the number of particle defects after the resist coating was counted in the same manner as in the evaluation of the developer and rinser.

[0388] <Pipe cleaning fluid evaluation>

[0389] The occurrence of defects when using chemical solutions (Examples 31 to 50 and 121 to 125, Comparative Examples 31 to 50 and 121 to 125) as pipe cleaning solutions was evaluated by the following method. The chemical solutions used in the evaluation of pipe cleaning solutions were the same as those used in the evaluation of the developer and rinse solution, the evaluation of the pre-wet solution, and the evaluation of the resist cleaning solution.

[0390] First, 7.57L (2 gallons) of liquid medicine was passed through the piping (PTFE) of the coating and developing device "CLEAN TRACK LITHIUS PRO-Z" manufactured by Tokyo Electron Co., Ltd. to clean the piping. The liquid medicine used in the cleaning of the piping was recovered. After that, the same liquid medicine used in the cleaning of the piping was applied to the silicon wafer through the piping of the coating and developing device. That is, the liquid medicine applied to the silicon wafer was the same liquid medicine used in the cleaning of the piping, and was not the liquid medicine used for the cleaning of the piping and recovered.

[0391] The number of particle defects after the resist coating was counted in the same manner as in the evaluation of the developer and rinser for the silicon wafers coated with the above chemical solutions.

[0392] <Results>

[0393] Tables 2 to 16 show the above-mentioned evaluation results.

[0394] In Tables 2 to 16, “Number of particle defects” indicates the number of defects per evaluated silicon wafer.

[0395] In Tables 2, 3, and 8 to 13, “number of pattern collapses” indicates the number of defects per evaluated silicon wafer.

[0396] [Table 2]

[0397]

[0398] [Table 3]

[0399]

[0400] [Table 4]

[0401]

[0402] [Table 5]

[0403]

[0404] [Table 6]

[0405]

[0406] [Table 7]

[0407]

[0408] [Table 8]

[0409]

[0410] [Table 9]

[0411]

[0412] [Table 10]

[0413]

[0414] [Table 11]

[0415]

[0416] [Table 12]

[0417]

[0418] [Table 13]

[0419]

[0420] [Table 14]

[0421]

[0422] [Table 15]

[0423]

[0424] [Table 16]

[0425]

[0426] <Analysis of Drug Solution>

[0427] In addition, each of the chemical solutions used in Examples and Comparative Examples was analyzed by the following method.

[0428] [Content of organic compounds other than organic solvents]

[0429] The content of organic compounds other than the organic solvent contained in the chemical solution was analyzed using a gas chromatograph-mass spectrometer (product name "GCMS-2020", manufactured by Shimadzu Corporation). The measurement conditions are as follows.

[0430] Capillary column: InertCap 5MS / NP, inner diameter 0.25 mm, length 30 m, film thickness 0.25 μ m

[0431] Sample introduction method: split flow, constant pressure (75kPa)

[0432] Vaporization chamber temperature: 230℃

[0433] Column oven temperature: 80℃(2min)-500℃(13min), heating rate 15℃ / min

[0434] Carrier gas: Helium

[0435] Septum purge flow rate: 5mL / min

[0436] Split ratio: 25:1

[0437] Inlet temperature: 250℃

[0438] Ion source temperature: 200°C

[0439] ·Measurement mode: Scan mode, m / z=85-500

[0440] Sample introduction volume: 1μ L

[0441] As a result of the above analysis, in each chemical solution, the total content of the organic compound other than the organic solvent was 0.1 to 1.0 ppm by mass relative to the total mass of the chemical solution.

[0442] [Metal content other than Fe, Ni and Zn]

[0443] The contents of metal components other than Fe, Ni, and Zn (other metal ions and other metal-containing particles) in the chemical solution were analyzed using ICP-MS.

[0444] Agilent 8900 manufactured by Agilent Technology was used as an analysis apparatus.

[0445] In each chemical solution, the content of other metal particles is 1 to 5 ppt by mass relative to the total mass of the chemical solution.

[0446] From the results of Tables 2, 3, and 14, it was confirmed that the chemical solutions of Examples 1 to 5, 6 to 10, 11 to 15, 16 to 20, and 106 to 110, whose I values ​​were not within the predetermined range, suppressed the occurrence of defects compared to the chemical solutions of Comparative Examples 1 to 5, 6 to 10, 11 to 15, 16 to 20, and 106 to 110, whose I values ​​were not within the predetermined range. More specifically, when used as a developer and a rinser, the chemical solutions of the comparative examples could not suppress either particle defects or pattern collapse, but the chemical solutions of the examples could suppress both.

[0447] From the results of Tables 4 and 15, it was confirmed that the chemical solutions of Examples 21 to 25, 111 to 115, and 116 to 120, whose I values ​​were not within the predetermined range, suppressed the occurrence of defects compared to the chemical solutions of Comparative Examples 21 to 25, 111 to 115, and 116 to 120, whose I values ​​were not within the predetermined range. More specifically, when used as a pre-wetting liquid, the chemical solutions of the comparative examples could not suppress either particle defects or resist coating unevenness, but the chemical solutions of the examples could suppress both.

[0448] The results in Table 5 show that the chemical solutions of Examples 26 to 30 whose I values ​​are within the predetermined range suppress the occurrence of defects, compared with the chemical solutions of Comparative Examples 26 to 30 whose I values ​​are not within the predetermined range. More specifically, when used as a resist cleaning solution, the chemical solutions of the comparative examples cannot suppress either particle defects or resist residues, but the chemical solutions of the examples can suppress both.

[0449] From the results of Tables 6, 7, and 16, it was confirmed that the chemical solutions of Examples 31 to 35, 36 to 40, 41 to 45, 46 to 50, and 121 to 125, whose I values ​​were not within the predetermined range, suppressed the occurrence of defects compared to the chemical solutions of Comparative Examples 31 to 35, 36 to 40, 41 to 45, 46 to 50, and 121 to 125, whose I values ​​were not within the predetermined range. More specifically, when used as a pipe cleaning solution, the chemical solutions of the comparative examples could not suppress particle defects, but the chemical solutions of the examples could suppress particle defects.

[0450] The results of Tables 8 to 13 show that the chemical solutions of Examples 51 to 105 whose I values ​​are within the predetermined range suppress the occurrence of defects, compared with the chemical solutions of Comparative Examples 51 to 105 whose I values ​​are not within the predetermined range. More specifically, when used as a developer for a metal resist, the chemical solutions of the comparative examples cannot suppress either particle defects or pattern collapse, but the chemical solutions of the examples can suppress both.

[0451] In addition, in Example 21, a mixed organic solvent of PGMEA and propylene glycol monomethyl ether (PGME) (mass ratio PGMEA:PGME=7:3) was used as the purified product instead of PGMEA, and the same purification was performed to obtain a drug solution. The same evaluation as in Example 21 was performed using the drug solution, and the results showed that the I value was 0.690 and the number of particle defects was 14.

[0452] Explanation of symbols

[0453] 33 Container

[0454] 36 Analysis Units

[0455] 38Carrier gas supply unit

[0456] 39Piping

[0457] 50Semiconductor substrate

[0458] 50a surface

[0459] 51 Containing metal particles

[0460] 51a Analytical sample

[0461] La laser light

Claims

1. A medicinal solution comprising: organic solvents; and containing metal particles comprising a metal element selected from the group consisting of Fe, Ni and Zn, The I value of the drug solution obtained by method X is 0.010 to 10.000, Method X: The sample is prepared by coating the liquid medicine on a substrate, and the surface of the sample is analyzed by scanning the laser using laser ablation-inductively coupled plasma-mass spectrometry, and a graph with the horizontal axis being the laser scanning time and the vertical axis being the ion detection intensity is obtained for each of the metal elements, and the ion detection intensity of the graph is accumulated according to the scanning time to obtain the accumulated ion detection intensity of each of the metal elements, and the accumulated ion detection intensity of each of the metal elements is summed up and set as the total accumulated ion detection intensity, and the total accumulated ion detection intensity is divided by the scanning area of ​​the laser to obtain the unit of counts / mm 2 The I value of .

2. The liquid medicine according to claim 1, wherein The chemical solution is one selected from the group consisting of a developer, a rinser, a pre-wet solution, a resist cleaning solution, and a pipe cleaning solution.

3. The liquid medicine according to claim 1 or 2, wherein: The organic solvent comprises butyl acetate, 4-methyl-2-pentanol, cyclohexanone, propylene glycol monomethyl ether acetate or isopropyl alcohol.

4. The liquid medicine according to claim 2, wherein: The liquid medicine is a developer, The organic solvent is selected from the group consisting of butyl acetate and 4-methyl-2-pentanol, or The organic solvent is a mixture of propylene glycol monomethyl ether acetate and a liquid organic acid.

5. The liquid medicine according to claim 2, wherein: The liquid medicine is a flushing liquid, The organic solvent is selected from the group consisting of butyl acetate, 4-methyl-2-pentanol and isopropanol.

6. The liquid medicine according to claim 2, wherein: The liquid medicine is a pre-wetting liquid. The organic solvent is selected from the group consisting of cyclohexanone, propylene glycol monomethyl ether acetate and isopropyl alcohol.

7. The liquid medicine according to claim 2, wherein: The liquid medicine is a resist cleaning liquid, The organic solvent is propylene glycol monomethyl ether acetate.

8. The liquid medicine according to claim 2, wherein: The liquid medicine is a pipe cleaning liquid. The organic solvent is selected from the group consisting of butyl acetate, 4-methyl-2-pentanol, cyclohexanone, isopropanol and propylene glycol monomethyl ether acetate.