Polyimide binder precursor composition and power storage device using same
By developing a polyimide binder precursor composition containing a high proportion of alicyclic tetracarboxylic dianhydride and aromatic diamine, the problem of large irreversible capacity in lithium-ion batteries has been solved and efficient lithium-ion charging has been achieved. discharge and mechanical strength, reducing battery weight and increasing capacity.
Patent Information
- Application Number
- CN202380026935.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-06-29
- Filing Date
- 2023-01-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-18
AI Technical Summary
The existing polyimide binder has a large irreversible capacity in lithium-ion batteries, which results in the lithium ions not being fully released during the charge and discharge process, increasing the weight and irreversible capacity of the battery, and the existing technology cannot effectively reduce the irreversible capacity. and optimized structure.
Develop a polyimide adhesive precursor composition that contains more than 50 mol% of alicyclic tetracarboxylic dianhydride and more than 50 mol% of an aromatic diamine compound. The polyimide produced through the imidization reaction Amine binder, with an irreversible capacity of less than 1200mAh/g, is used to prepare the negative active material layer, reducing the amount of active material on the positive electrode side, and improving the capacity and efficiency of the battery.
Achieved high initial charge and discharge efficiency of lithium-ion secondary batteries, reduced the amount of active material on the positive electrode side, and obtained a light-weight and high-capacity power storage device. The polyimide binder has excellent mechanical properties and can Withstand volume changes in electrode materials and prevent active materials from falling off.
Smart Images

Figure BDA0005038020780000051 
Figure BDA0005038020780000061 
Figure BDA0005038020780000081
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide-based adhesive for use in power storage devices such as lithium ion secondary batteries, and more particularly to a polyimide adhesive precursor composition, an electrode mixture paste, a negative electrode active material layer, a negative electrode sheet, and a power storage device. Background Art
[0002] Power storage devices such as lithium secondary batteries have high energy density and high capacity, and are therefore widely used as driving power sources for mobile information terminals. In recent years, applications for industrial use (e.g., mounted on electric / hybrid vehicles and unmanned aerial vehicles, etc.) have been studied, and further increases in the capacity of power storage devices are being promoted. As an example of increasing capacity, with respect to the negative electrode constituting the power storage device, research has been conducted to increase the charge and discharge capacity by using silicon or tin having a large storage capacity per unit volume, or alloys containing these.
[0003] However, it is known that electrode active materials having a large charge and discharge capacity (such as silicon or tin or alloys containing these) cause very large volume changes associated with charge and discharge. Therefore, when these electrode active materials are used to form a negative electrode active material layer using a general-purpose binder such as polyvinylidene fluoride or a rubber-based resin, problems such as collapse of the negative electrode active material layer or interface peeling between the current collector and the negative electrode active material layer may occur due to the volume change of the electrode active material, thereby causing deterioration in the cycle characteristics of the power storage device.
[0004] In order to solve these problems, the use of a polyimide-based binder has been proposed as a method for improving the degradation of cycle characteristics caused by volume change during repeated charge and discharge (for example, see Patent Documents 1 to 3).
[0005] On the other hand, Patent Document 4 (US2006 / 0099506) points out that when a polyimide-based adhesive is used, a larger irreversible capacity can be observed. Specifically, Patent Document 4 proposes a solution for reducing the irreversible capacity in a polyimide-based adhesive obtained from 3,3'4,4'-benzophenonetetracarboxylic dianhydride and 4,4'-oxydianiline by replacing part or all of the tetracarboxylic dianhydride with 1,2,3,4-butanetetracarboxylic dianhydride (open-chain aliphatic tetracarboxylic dianhydride).
[0006] In addition, Patent Document 5 (JP 2019-3873A) describes the use of a binder of a polymer compound containing an imide group in a negative electrode active material layer containing a silicon-based negative electrode active material, wherein the binder has a tensile elastic modulus of 3.0 GPa or more and a reactivity to lithium ions of 1200 mAh / g or less.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: WO 2013 / 035806
[0010] Patent Document 2: WO 2017 / 022796
[0011] Patent Document 3: WO 2018 / 174299
[0012] Patent Document 4: US2006 / 0099506
[0013] Patent Document 5: Japanese Patent Application Publication No. 2019-3873 Summary of the invention
[0014] Technical issues
[0015] The inventors have found that if the binder itself has irreversible capacity, then during the first charge, lithium will also be taken into the binder, and during discharge, the lithium will remain in the binder and will not be released, so lithium exceeding the theoretical capacity of the negative electrode active material is required.
[0016] Therefore, the greater the irreversible capacity of the adhesive itself, the more lithium must be loaded on the positive electrode, which may increase the weight of the entire battery. In order to eliminate these problems, it is necessary to develop a polyimide adhesive with a smaller irreversible capacity. As mentioned above, the purpose of Patent Document 4 is to reduce the irreversible capacity, but the degree of reduction is not enough and the composition is not considered. In addition, Patent Document 5 believes that the reactivity to lithium ions is related to the cycle characteristics, but the initial irreversible capacity is not measured. In order to correctly evaluate the impact on the initial efficiency, it is necessary to evaluate the charge and discharge capacity of the adhesive itself and estimate the irreversible capacity as the difference between the two. And the structure of the polyimide is hardly mentioned, so the details cannot be understood.
[0017] Furthermore, in the case of a lithium ion capacitor, if the irreversible capacity of the binder is large, a large amount of lithium ions will be required for pre-doping, and it is expected that the pre-doping treatment time and the like will vary significantly.
[0018] The present invention aims to solve the above problems and has the object of providing a polyimide binder having a small irreversible capacity and a precursor composition thereof. In addition, by using the polyimide binder of the present invention, a storage device such as a lithium ion secondary battery having a high initial charge and discharge efficiency can be provided.
[0019] Technical Solution
[0020] The present invention relates to the following items.
[0021] 1. A polyimide binder precursor composition for an electrode of a storage device, comprising a reaction product of a tetracarboxylic acid component and a diamine component and a solvent,
[0022] The irreversible capacity of the polyimide adhesive obtained from the polyimide adhesive precursor composition is less than or equal to 1200 mAh / g.
[0023] 2. The polyimide adhesive precursor composition according to item 1 above, comprising a reaction product of a tetracarboxylic acid component containing 50 mol % or more of alicyclic tetracarboxylic dianhydride and a diamine component, and a solvent.
[0024] 3. The polyimide adhesive precursor composition according to item 1 or 2 above, wherein the diamine component contains 50 mol % or more of an aromatic diamine compound.
[0025] 4. A negative electrode mixture paste for an electrical storage device, comprising the polyimide binder precursor composition according to any one of items 1 to 3 above and an active material containing a silicon-containing material and / or graphite.
[0026] 5. A negative electrode for an electric storage device, comprising:
[0027] (a) an electrode active material layer, comprising an active material containing a silicon-containing material and / or graphite and a polyimide binder, wherein the polyimide binder is a heating product of a polyimide precursor in the polyimide binder precursor composition described in any one of items 1 to 3 above; the polyimide binder binds the active material; and
[0028] (b) Current collector.
[0029] 6. An electricity storage device comprising the negative electrode for an electricity storage device according to item 5 above.
[0030] 7. A method for manufacturing a negative electrode for an electric storage device, comprising the following steps:
[0031] Casting or coating the negative electrode mixture paste described in item 4 above onto a current collector; and
[0032] The coated layer of the negative electrode mixture paste is heated to form a negative electrode active material layer.
[0033] 8. A method for manufacturing an electricity storage device, comprising the method for manufacturing a negative electrode as described in the above item 7 as a step.
[0034] Beneficial Effects
[0035] According to the present invention, a polyimide adhesive having a small irreversible capacity and a precursor composition thereof are provided. In addition, by using the polyimide adhesive of the present invention, a storage device such as a lithium ion secondary battery having a high initial charge and discharge efficiency can be provided. For example, when the polyimide adhesive is used as a negative electrode adhesive, the amount of active material on the positive electrode side that compensates for the irreversible capacity can be reduced, thereby being able to obtain a light-weight and high-capacity storage device. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a diagram showing one embodiment of a method for calculating the irreversible capacity of the polyimide adhesive itself in the present invention. DETAILED DESCRIPTION
[0037] The polyimide adhesive precursor composition of the present invention comprises a reaction product of a tetracarboxylic acid component and a diamine component and a solvent. The reaction product of the tetracarboxylic acid component and the diamine component in the polyimide adhesive precursor composition is a polyimide precursor described below. The polyimide adhesive precursor composition of the present invention can be converted into a polyimide adhesive that binds active material particles, for example, by heating the polyimide adhesive precursor composition of the present invention together with, for example, active material particles to remove the solvent, and then, if necessary, the polyimide adhesive precursor composition is subjected to imidization reaction. Therefore, in the present invention, "polyimide adhesive" (of the present invention) refers to an adhesive obtained by the polyimide adhesive precursor composition of the present invention, and is a substance that binds active material particles in, for example, an electrode.
[0038] The irreversible capacity of the polyimide adhesive obtained from the polyimide adhesive precursor composition of the present invention is 1200 mAh / g or less, preferably 1100 mAh / g or less, more preferably 1000 mAh / g or less, more preferably 900 mAh / g or less, and even more preferably 800 mAh / g or less.
[0039] The irreversible capacity of the polyimide adhesive can be determined in the following manner.
[0040] (1) A polyimide binder precursor composition and a negative electrode active material were mixed at different ratios to prepare a plurality of evaluation mixture pastes. Using these evaluation mixture pastes, a plurality of evaluation negative electrodes having different polyimide binder content ratios were manufactured.
[0041] (2) For example, using metallic lithium as a counter electrode, the initial charge capacity and initial discharge capacity of the negative electrode for evaluation are measured, and the difference between the charge capacity (mAh / g) and the discharge capacity (mAh / g) of the active material layer is defined as the irreversible capacity (mAh / g) of the negative electrode for evaluation. Here, the charge capacity and discharge capacity per unit mass are calculated based on the total mass of the active material and the binder.
[0042] (3) The irreversible capacity (mAh / g) of the negative electrode for evaluation was plotted against the content (mass %) of the polyimide binder to create a calibration curve. The irreversible capacity of the negative electrode for evaluation with a polyimide binder content of 100% was defined as the "irreversible capacity of the polyimide binder".
[0043] The negative electrode active material used to make the negative electrode for evaluation does not need to be a silicon-based material, and graphite is preferably used, and the capacity of graphite is smaller than that of silicon-based materials. In addition, in order to eliminate the influence of the irreversible capacity of the counter electrode, the counter electrode is preferably made of metallic lithium.
[0044] It is also preferred that the polyimide binder has excellent mechanical properties. Even if a material that undergoes a large volume change, such as a silicon-based material, is used as an electrode active material, a binder having excellent mechanical properties can withstand expansion and contraction during charge and discharge, and is therefore known to prevent the active material from falling off, thereby having excellent cycle characteristics.
[0045] Mechanical properties of the polyimide adhesive may be measured using a polyimide film formed from the polyimide adhesive precursor composition.
[0046] The representative mechanical property is the elastic modulus, which is preferably 1.0 GPa or more, more preferably 2.0 GPa or more, and even more preferably 2.5 GPa or more. The elongation (breaking elongation) is also preferably large, specifically, preferably 30% or more, more preferably 40% or more, even more preferably 50% or more, even more preferably 60% or more, and even more preferably 70% or more. The breaking energy is preferably 40 MJ / m 3 More preferably 50MJ / m 3 More preferably 60MJ / m 3 above.
[0047] In particular, it is preferred that the elastic modulus, elongation (elongation at break), and breaking energy all satisfy the "preferred" ranges simultaneously.
[0048] Next, the components and production method of the polyimide adhesive precursor composition will be described.
[0049] <Reaction product of tetracarboxylic acid component and diamine component>
[0050] In this specification, tetracarboxylic acid component includes tetracarboxylic acid, tetracarboxylic dianhydride and other tetracarboxylic acid derivatives, such as tetracarboxylic acid silyl ester, tetracarboxylic ester and tetracarboxylic acid chloride, which are used as raw materials for making polyimide. Although not particularly limited, from the perspective of manufacturing, it is convenient to use tetracarboxylic dianhydride, and the example of using tetracarboxylic dianhydride as tetracarboxylic acid component will be mainly described below. In addition, diamine component is a diamine compound with two amino groups (-NH2) used as the raw material for making polyimide.
[0051] Here, the reaction product of the tetracarboxylic acid component and the diamine component is generally referred to as a polyimide precursor, and generally includes a polyamic acid (or its derivative) whose repeating unit is represented by the following general formula (I), but may also have a structure that is further imidized. In the formula, X1 is derived from the tetracarboxylic acid component, and Y1 is derived from the diamine component.
[0052]
[0053] (Wherein, in the general formula I, X1 is a tetravalent aliphatic group or an aromatic group, Y1 is a divalent aliphatic group or an aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms).
[0054] The further imidized repeating unit of the general formula (I) is a structure in which one or both of the two amide bonds present in the general formula (I) are converted into imide bonds, and is specifically represented by the following general formulas (Ib), (Ic) and (II):
[0055]
[0056] If each repeating unit in the polyimide precursor has the general formula (I), the imidization rate is 0%; if each repeating unit has the general formula (Ib) and / or (Ic), the imidization rate is 50%; if each repeating unit has the general formula (II), the imidization rate is 100% (i.e., polyimide). The imidization rate of the polyimide precursor may be in any range of 0 to 100%. In the present application, even if the imidization rate is 100%, those present in the polyimide adhesive precursor composition are still referred to as polyimide precursors.
[0057] In a preferred embodiment, the polyimide precursor comprises a repeating unit of formula (I), for example, it may comprise a repeating unit selected from formula (I), (Ib) and / or (Ic) and formula (II), so that the imidization rate is 0% to 50%, for example, 0% to 30%, or further 0% to 20%. In another embodiment, the polyimide precursor comprises a repeating unit of formula (II), for example, it may comprise a repeating unit selected from the above formula, so that the imidization rate is greater than 50% to 100%.
[0058] As the tetracarboxylic acid component, an aliphatic tetracarboxylic dianhydride or an aromatic tetracarboxylic dianhydride can be used. As the aliphatic tetracarboxylic dianhydride, an alicyclic tetracarboxylic dianhydride is preferred, for example, a tetracarboxylic dianhydride in which four carboxyl groups are directly bonded to X1 as an alicyclic group is preferred. The use of an alicyclic tetracarboxylic dianhydride can achieve both high capacity and mechanical strength of the storage device by reducing the irreversible capacity of the polyimide binder.
[0059] In a preferred embodiment of the present invention, the proportion of alicyclic tetracarboxylic dianhydride in the total tetracarboxylic acid components is 50 mol% or more, more preferably 60 mol% or more, even more preferably 70 mol% or more, even more preferably 80 mol% or more (including 100 mol%). The remaining tetracarboxylic acid components are preferably aromatic tetracarboxylic dianhydride.
[0060] When the polyimide precursor is obtained using a tetracarboxylic acid component containing alicyclic tetracarboxylic dianhydride and other tetracarboxylic dianhydride (preferably aromatic tetracarboxylic dianhydride), its form is not limited, and it can be a copolymer, a block (co)polymer, a blend of homopolymers, or a blend of copolymers and homopolymers. The copolymer contains X1 as an alicyclic group and X1 as an aromatic group in one molecule. The block (co)polymer is formed by reacting a block having a repeating unit of X1 as an alicyclic group and a block having a repeating unit of X1 as an aromatic group to form one molecule. A homopolymer blend is a blend of a polymer having only X1 as an alicyclic group and a polymer having only X1 as an aromatic group.
[0061] For the purpose of explaining the alicyclic tetracarboxylic dianhydride, the alicyclic group X1 is preferably a tetravalent group having an alicyclic structure having a carbon number of 4 to 40, more preferably having at least one aliphatic 4-membered to 12-membered ring, more preferably an aliphatic 4-membered ring or an aliphatic 6-membered ring. Preferred examples of the tetravalent group having an aliphatic 4-membered ring or an aliphatic 6-membered ring include the following groups.
[0062]
[0063] (Among them, R 31 To R 38 Each independently is a direct bond or a divalent organic group, R 41 To R 47 and R 71 To R 73 Each independently represents one selected from the group consisting of groups represented by the following formulae: -CH2-, -CH=CH-, -CH2CH2-, -O- and -S-. 48 is an organic group having an aromatic ring or an alicyclic structure).
[0064] R 31 , R 32 , R 33 , R 34 , R 35 , R 36 , R 37 and R 38Specific examples include a direct bond, an organic group having an aromatic ring or an alicyclic structure, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, or an oxygen atom (—O—), a sulfur atom (—S—), a carbonyl bond, an ester bond, and an amide bond.
[0065] Contains R 31 To R 38 or R 48 Examples of the organic group of the aromatic ring include the following groups.
[0066]
[0067] (W1 is a direct bond or a divalent organic group; n11 to n13 each independently represent an integer from 0 to 4; R 51 , R 52 and R 53 Each is independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group or a trifluoromethyl group).
[0068] Specific examples of W1 include a divalent group represented by the following formula (5) and a divalent group represented by the following formula (6).
[0069]
[0070] (where R in formula (6) 61 To R 68 Each independently represents any one of the divalent groups represented by formula (5).
[0071] Among them, as the tetravalent group having an alicyclic structure, the following groups are particularly preferred.
[0072]
[0073] Examples of tetracarboxylic dianhydrides include: monocyclic alicyclic tetracarboxylic dianhydrides such as 1,2,3,4-cyclobutanetetracarboxylic dianhydride and cyclohexane-1,2,4,5-tetracarboxylic dianhydride; and alicyclic tetracarboxylic dianhydrides having two or more rings such as [1,1'-bis(cyclohexane)]-3,3',4,4'-tetracarboxylic dianhydride, [1,1'-bis(cyclohexane)]-2,3,3',4'-tetracarboxylic dianhydride, [1,1'-bis(cyclohexane)]-2,2',3,3'-tetracarboxylic dianhydride, 4,4'-methylenebis(cyclohexane-1,2-dicarboxylic dianhydride), 4,4'-(propane-2, 2-diyl)bis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-oxybis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-thiobis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-sulfonylbis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-(dimethylsilanediyl)bis(cyclohexane-1,2-dicarboxylic anhydride), 4,4'-(tetrafluoropropane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic anhydride), octahydropentalene-1,3,4,6-tetracarboxylic anhydride, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic anhydride, 6-(carboxymethyl) ) bicyclo[2.2.1]heptane-2,3,5-tricarboxylic dianhydride, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic dianhydride, bicyclo[2.2.2]oct-5-ene-2,3,7,8-tetracarboxylic dianhydride, tricyclo[4.2.2.02,5]decane-3,4,7,8-tetracarboxylic dianhydride, tricyclo[4.2.2.02,5]dec-7-ene-3,4,9,10-tetracarboxylic dianhydride, 9-oxatricyclo[4.2.1.02,5]nonane-3,4,7,8-tetracarboxylic dianhydride, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane Pyranane-5,5",6,6"-tetracarboxylic dianhydride, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethylnaphthalene-2c,3c,6c,7c-tetracarboxylic dianhydride, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethylnaphthalene-2t,3t,6c,7c-tetracarboxylic dianhydride, decahydro-1,4-ethyl-5,8-methylnaphthalene-2,3,6,7-tetracarboxylic dianhydride, tetradecahydro-1,4:5,8:9,10-trimethylanthracene-2,3,6,7-tetracarboxylic dianhydride, etc. These can be used alone or in combination of two or more.
[0074] The aromatic tetracarboxylic dianhydride preferably has 2 to 3 aromatic rings. Examples of the aromatic group X1 include compounds having the following structures.
[0075]
[0076] (Wherein Z1 is a direct bond, or any of the following divalent groups:
[0077]
[0078] Wherein, Z2 in the formula is a divalent organic group, Z3 and Z4 are each independently an amide bond, an ester bond and a carbonyl bond, and Z5 is an organic group containing an aromatic ring).
[0079] Specific examples of Z2 include aliphatic hydrocarbon groups having 2 to 24 carbon atoms and aromatic hydrocarbon groups having 6 to 24 carbon atoms.
[0080] Specific examples of Z5 include aromatic hydrocarbon groups having 6 to 24 carbon atoms.
[0081] Examples of preferred aromatic tetracarboxylic dianhydrides include, but are not limited to, halogen-unsubstituted aromatic tetracarboxylic dianhydrides, such as 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, pyromellitic dianhydride, benzophenonetetracarboxylic dianhydride, 4,4'-oxydiphthalic dianhydride, diphenylsulfonetetracarboxylic dianhydride, p-terphenyltetracarboxylic dianhydride, m-terphenyltetracarboxylic dianhydride; and
[0082] Halogen-substituted tetracarboxylic dianhydrides, such as 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 3,3'-(hexafluoroisopropylidene)diphthalic anhydride, 5,5'-[2,2,2-trifluoro-1-[3-(trifluoromethyl)phenyl]ethylidene]diphthalic anhydride, 5,5'-[2,2,3,3,3-pentafluoro-1-(trifluoromethyl)propylene]diphthalic anhydride, 1H-difluoro[3,4-b:3',4'-i]xanthene-1,3,7,9(11H)-tetraone, 5,5'-oxybis[4,6,7-trifluoro-pyromellitic anhydride], 3,6-bis(trifluoromethyl)pyromellitic dianhydride, 4-(trifluoromethyl)pyromellitic dianhydride, 1,4-difluoropyromellitic dianhydride, 1,4-bis(3,4-dicarboxytrifluorophenoxy)tetrafluorophthalic anhydride, etc. These can be used alone or in combination of two or more.
[0083] As the diamine component, an aromatic diamine compound or an aliphatic diamine compound can be used. In a preferred embodiment of the present invention, the proportion of the aromatic diamine compound in the total diamine component is 50 mol% or more, more preferably 60 mol% or more, even more preferably 70 mol% or more, even more preferably 80 mol% or more (including 100 mol%). The remaining diamine components are aliphatic diamine compounds, preferably diamine compounds with alicyclic structures. In another different embodiment, the diamine component may contain an aliphatic diamine compound, preferably an alicyclic diamine compound, based on the total diamine components, a ratio of 50 mol% or more, more preferably 60 mol% or more, even more preferably 70 mol% or more, even more preferably 80 mol% or more (including 100 mol%).
[0084] To illustrate the aromatic diamine compound, examples of the aromatic group Y1 include the following.
[0085]
[0086] (W1 is a direct bond or a divalent organic group; n11 to n13 each independently represent an integer from 0 to 4; R 51 , R 52 and R 53 Each is independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group or a trifluoromethyl group).
[0087] Specific examples of W1 include a divalent group represented by the following formula (5) and a divalent group represented by the following formula (6).
[0088]
[0089] (Wherein, R in formula (6) 61 To R 68 Each independently represents any one of the divalent groups represented by formula (5).
[0090] Examples of the diamine component providing a repeating unit in which Y1 in the general formula (I) is a divalent group having an aromatic ring include p-phenylenediamine, m-phenylenediamine, 2,4-toluenediamine, 3,3'-dihydroxy-4,4'-diaminobiphenyl, bis(4-amino-3-carboxyphenyl)methane, benzidine, 3,3'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, m-tolidine, 4,4'-diaminobenzanilide, 3,4'-diaminobenzanilide, N,N'-di(4-aminophenyl)terephthalamide, N,N'-di(p-aminobenzamide) ), 4-aminophenoxy-4-diaminobenzoate, bis(4-aminophenyl) terephthalate, biphenyl-4,4'-dicarboxylic acid bis(4-aminophenyl) ester, p-phenyl di(p-aminobenzoate), bis(4-aminophenyl)-[1,1'-biphenyl]-4,4'-dicarboxylate, [1,1'-biphenyl]-4,4'-diyl di(4-aminobenzoate), 4,4'-oxydiphenylamine (also known as 4,4'-diaminodiphenyl ether), 3,4'-oxydiphenylamine, 3,3'-oxydiphenylamine, p-methylenebis(phenylenediamine), 1,3-bis(4-aminophenoxy)benzene, 1,3-bis(3 2,2-bis(4-aminophenyl)propane, bis(4-aminophenyl)sulfone, 2,2-bis(4-aminophenyl)hexafluoropropane, bis(4-aminophenyl)sulfone, 3,3'-bis(trifluoromethyl)benzidine, 3,3'-bis((aminophenoxy)phenyl)propane, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(4-(4-aminophenyl)propane)hexafluoropropane, bis(4-aminophenyl)sulfone, 2,2-bis(4-aminophenyl)hexafluoropropane, bis(4-aminophenyl)sulfone, 3,3'-bis(trifluoromethyl)benzidine, 3,3'-bis((aminophenoxy)phenyl)propane, 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(4-(4-aminophenyl) bis(4-(3-aminophenoxy)diphenyl)sulfone, bis(4-(3-aminophenoxy)diphenyl)sulfone, octafluorobenzidine, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 2,4-bis(4-aminoanilino)-6-amino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-methylamino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-ethylamino-1,3,5-triazine and 2,4-bis(4-aminoanilino)-6-anilino-1,3,5-triazine. Examples of the diamine component providing a repeating unit in which Y1 in the general formula (I) is a divalent group having an aromatic ring containing a fluorine atom include 2,2′-bis(trifluoromethyl)benzidine, 3,3′-bis(trifluoromethyl)benzidine, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane and 2,2′-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.In addition, preferred diamine compounds include 9,9-bis(4-aminophenyl)fluorene, 4,4′-(((9H-fluorene-9,9-diyl)bis([1,1′-biphenyl]-5,2-diyl))bis(oxy))diamine, [1,1′:4′,1″-terphenyl]-4,4″-diamine, and 4,4′-([1,1′-binaphthyl]-2,2′-diylbis(oxy))diamine. The above diamine components can be used alone or in combination of multiple types.
[0091] In order to illustrate the diamine compound having an alicyclic structure, examples of Y1 as a group having an alicyclic structure include the following.
[0092]
[0093] (Wherein, V1 and V2 are each independently a direct bond or a divalent organic group; n 21 to n 26 Each independently represents an integer from 0 to 4; R 81 To R 86 are each independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group or a trifluoromethyl group; and R 91 , R 92 and R 93 Each independently selected from the group consisting of groups represented by the following formulae: -CH2-, -CH=CH-, -CH2CH2-, -O- and -S-
[0094] Specific examples of V1 and V2 include a direct bond and a divalent group represented by the above-mentioned formula (5).
[0095] Examples of the diamine component providing a repeating unit in which Y1 in the general formula (I) is a divalent group having an alicyclic structure include 1,4-diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-tert ... Cyclobutane, 1,4-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, diaminobicycloheptane, diaminomethylbicycloheptane, diaminooxybicycloheptane, diaminomethoxybicycloheptane, isophoronediamine, diaminotricyclodecane, diaminomethyltricyclodecane, di(aminocyclohexyl)methane, di(aminocyclohexyl)isopropane, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane and 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane. These diamine components may be used alone or in combination of two or more.
[0096] [Solvent]
[0097] Preferred examples of the solvent include non-polar solvents (solvents having a dielectric constant of 6 or less), including: aromatic hydrocarbons such as xylene, toluene and ethylbenzene, aliphatic hydrocarbons such as pentane, hexane and heptane, and benzoic acid esters such as methyl benzoate, ethyl benzoate and propyl benzoate; polar solvents (solvents having a dielectric constant greater than 6), including water, methanol, ethanol, acetone, N,N-dimethylformamide, dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methyl-2-pyrrolidone, N-ethyl The solvents include, for example, 1,2-dimethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, hexamethylphosphoric triamide, 1,2-dimethoxymethane, bis(2-methoxyethyl)ether, 1,2-bis(2-methoxyethoxy)ethane, tetrahydrofuran, bis[2-(2-methoxyethoxy)ethyl]ether, 1,4-dioxane, dimethyl sulfoxide, dimethyl sulfone, diphenyl ether, cyclopentane, diphenyl sulfone, tetramethylurea, anisole, m-cresol, phenol, γ-butyrolactone, and mixtures thereof. In particular, water, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and γ-butyrolactone are preferred.
[0098] <Polyimide Adhesive Precursor Composition>
[0099] The polyimide adhesive precursor composition of the present invention is obtained by reacting a tetracarboxylic acid component and a diamine component in a reaction solvent. The reaction solvent may be any of the above-mentioned solvents, and the reaction solvent is preferably contained in the polyimide adhesive precursor composition as it is.
[0100] The reaction is carried out at a relatively low temperature using approximately equimolar amounts of tetracarboxylic acid components (tetracarboxylic dianhydride) and diamine components, for example, above 25°C and below 100°C, preferably below 80°C. Although not limited thereto, the reaction temperature is generally 25°C to 100°C, preferably 25°C to 80°C, more preferably 30°C to 80°C, for example, the reaction time is about 0.1 hour to 72 hours, preferably 2 hours to 60 hours. The reaction can be carried out under an air atmosphere, but is generally suitable for being carried out in an inert gas atmosphere, preferably a nitrogen atmosphere.
[0101] Here, approximately equimolar amounts of the tetracarboxylic acid component (tetracarboxylic dianhydride) and the diamine component specifically means that the molar ratio of [tetracarboxylic acid component / diamine component] is about 0.90 to 1.10, preferably about 0.95 to 1.05.
[0102] The solid content concentration of the polyimide adhesive precursor composition (polyimide conversion concentration of the polyimide precursor) is preferably greater than 5% to 45% by mass, more preferably greater than 10% to 40% by mass, and more preferably greater than 10% to 30% by mass. When the solid content concentration is less than 5% by mass, the viscosity of the composition becomes too low; when the solid content concentration is higher than 45% by mass, the composition may lose fluidity. The reaction solution of the tetracarboxylic acid component and the diamine component can be directly used as a polyimide adhesive precursor composition, or the concentration can be adjusted by concentration or dilution when necessary.
[0103] As for the solution viscosity (viscosity of the polyimide binder precursor composition), the solution viscosity at 30° C. is preferably 1000 Pa·sec or less, more preferably 500 Pa·sec or less, further preferably 300 Pa·sec or less, and particularly preferably 200 Pa·sec or less. The solution viscosity is preferably 1000 Pa·sec or less because it is beneficial to mix the electrode active material powder and uniformly coat it on the current collector.
[0104] The polyimide binder precursor composition may contain additives other than the electrode active material, and these additives will be described in the next section "Electrode mixture paste". The following is a detailed description using a lithium ion secondary battery as an example.
[0105] <Electrode Mixture Paste>
[0106] The electrode mixture paste as one embodiment of the present invention is a composition including a polyimide binder precursor composition, an electrode active material, and an optionally added solvent.
[0107] As the electrode active material that can be used for the electrode mixture paste of the present invention, known materials can be preferably used. The polyimide binder precursor composition of the present invention can be used for the negative electrode or the positive electrode. Therefore, the electrode active material can be a negative electrode active material or a positive electrode active material. Generally, the negative electrode is more effective in using the polyimide binder precursor composition of the present invention. In this case, the electrode active material comprises a negative electrode active material. For example, as the electrode active material, preferably a metal composite oxide, carbon powder, silicon powder, tin powder or an alloy powder containing silicon or tin containing lithium. The amount of the electrode active material in the electrode mixture paste is not particularly limited and can be appropriately determined according to the required capacity. Generally, based on the mass reference amount of the solid content (polyimide conversion mass) in the polyimide binder precursor composition, the amount of the electrode active material is preferably 0.1 times or more, more preferably 1 times or more, more preferably 5 times or more, and more preferably 10 times or more. Within these ranges, more active parts are contained in the negative electrode active material layer, which enables it to act as an electrode satisfactorily. On the other hand, in order to sufficiently bind the electrode active material to the current collector and effectively prevent it from falling off, the amount of the electrode active material is generally preferably 1000 times or less of the solid content in the polyimide binder precursor composition.
[0108] As negative electrode active materials for lithium secondary batteries, lithium metal, lithium alloys, carbon materials capable of absorbing and releasing lithium [easily graphitized carbon, non-graphitized carbon with a (002) plane spacing of 0.37 nm or more, or graphite with a (002) plane spacing of 0.34 nm or less], tin (single substance), tin compounds, silicon (single substance), silicon compounds, or lithium titanate compounds (e.g., Li4Ti5O 12 ) etc. can be used alone or in combination of two or more. In the present invention, it is preferred that the negative electrode active material at least comprises tin (single substance), tin compound, silicon-containing material (in the following description, referred to as silicon-containing negative electrode active material or silicon-containing material), such as silicon (single substance) or silicon compound. In particular, compared with graphite, silicon-containing materials such as silicon (single substance) or silicon compounds have extremely large theoretical capacity, and the volume expansion rate of the electrode active material itself during charging is also extremely large.
[0109] The lithium ion secondary battery using the polyimide binder precursor composition of the present invention can suppress the degradation of the electrode active material due to volume expansion, and is excellent not only in the characteristics during use (such as cycle characteristics) but also in the characteristics over a wide temperature range (such as low temperature characteristics or gas generation after high temperature storage).
[0110] The type of the silicon-containing active material is not particularly limited, and examples thereof include silicon (elemental), silicon compounds, partially substituted products of silicon, partially substituted products of silicon compounds, and solid solutions of silicon compounds. Specific suitable examples of the silicon compounds include silicon oxides represented by the formula: SiOx (0.05 < x < 1.95), silicon carbides represented by the formula: SiCy (0 < y < 1), silicon nitrides represented by the formula: SiNz (0 < z < 4 / 3), and silicon alloys which are alloys of silicon and other different elements M. In the case of the silicon alloy, preferred examples of the other different element M1 include at least one element selected from the group consisting of Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn, and Ti.
[0111] The partially substituted product of silicon is a compound in which a part of the silicon contained in silicon (elemental) and silicon compounds is substituted by other different elements M2. Specific preferred examples of the other different element M2 include B, Mg, Ni, Ti, Mo, Co, Ca, Cr, Cu, Fe, Mn, Nb, Ta, V, W, Zn, C, N, and Sn. Among these silicon-containing active materials, silicon (elemental), silicon oxides, and silicon alloys are more preferred, and silicon (elemental) and silicon oxides are further more preferred.
[0112] In order to obtain a higher capacity, the amount of the silicon-containing active material is preferably 1% by mass or more, more preferably 5% by mass or more, still more preferably 10% by mass or more, based on the mass of the net silicon in the negative electrode mixture, and from the perspective of improving the cycle characteristics, it is preferably 95% by mass or less, more preferably 65% by mass or less, still more preferably 45% by mass or less.
[0113] Preferred solvents that can be used in the electrode mixture paste include: non-polar solvents such as aromatic hydrocarbons, such as xylene, toluene, and ethylbenzene, aliphatic hydrocarbons, such as pentane, hexane, and heptane, and benzoates, such as methyl benzoate, ethyl benzoate, and propyl benzoate; and water, methanol, ethanol, acetone, N,N-dimethylformamide, dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, N-methylcaprolactam, hexamethylphosphoric triamide, 1,2-dimethoxymethane, bis(2-methoxyethyl) ether, 1,2-bis(2-methoxyethoxy)ethane, tetrahydrofuran, bis[2-(2-methoxyethoxy)ethyl] ether, 1,4-dioxane, dimethyl sulfoxide, dimethyl sulfone, diphenyl ether, sulfolane, diphenyl sulfone, tetramethylurea, anisole, m-cresol, phenol, γ-butyrolactone; in particular, water, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, and γ-butyrolactone are preferred.
[0114] As the solvent, the solvent in the polyimide adhesive precursor composition may be used directly, or may be concentrated or another solvent may be added if necessary so as to provide an appropriate coating concentration.
[0115] In the electrode mixture paste of the present invention, when it is an aqueous solvent system, it is preferably contained a pyridine compound or an imidazole compound. Therefore, the swelling degree of the obtained polyimide relative to the electrolyte can be made smaller, and the elongation (elongation at break) and the fracture energy can be made larger. In addition, the heat treatment temperature for obtaining the negative electrode active material layer can be reduced. The pyridine compound is a compound having a pyridine portion in its chemical structure, and preferred examples thereof include pyridine, 3-pyridinol, quinoline, isoquinoline, quinoxaline, 6-tert-butylquinoline, acridine, 6-quinolinecarboxylic acid, 3,4-dimethylpyridine and pyridazine. These pyridine compounds can be used alone or in combination of two or more. Examples of imidazole compounds include 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 4-ethyl-2-methylimidazole and 1-methyl-4-ethylimidazole, etc. Imidazoles can be used alone or in a mixture of multiple.
[0116] The addition amount of pyridine compound is not limited, but relative to 1mol of the repeating unit of polyimide precursor (particularly polyamic acid), preferably 0.05 to 2.0 molar equivalents, more preferably 0.1 to 1.0 molar equivalents. If the addition amount is outside the scope, it may be difficult to use an aqueous solvent system. The addition amount of imidazole compound is not limited, but relative to the amic acid repeating unit of 1mol of polyamic acid is more than 1.6 molar equivalents, more preferably more than 2.0 molar equivalents, and more preferably more than 2.4 molar equivalents.
[0117] If necessary, known additives may be added to the electrode mixture paste of the present invention. For example, negative electrode conductive agents, alkalis, surfactants, viscosity modifiers, conductive aids, silane coupling agents, adhesives other than polyimide adhesives, etc. may be used, as long as the effect of the present invention is not impaired.
[0118] The negative electrode conductive agent is not particularly limited as long as it is an electronic conductive material that does not cause chemical changes, but it is preferred to use a metal powder (such as copper, nickel, titanium or aluminum) or a carbon material, etc. The carbon material used as the conductive agent and the negative electrode active material preferably includes: graphite, such as natural graphite (flaky graphite, etc.), artificial graphite and other graphites; one or more carbon blacks selected from acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; and fibrous carbon powders, such as carbon nanotubes and carbon fibers.
[0119] In addition, it is more preferred that the negative electrode conductive agent can be appropriately mixed and used in a mixture, such as graphite and carbon black, graphite and fibrous carbon powder, or carbon black and fibrous carbon powder. In particular, fibrous carbon powder is preferably used because it has the effect of reducing the use of a conductive agent with a larger specific surface area to ensure conductivity. The carbon material is used as a conductive agent or a negative electrode active material, and the amount of the carbon material added to the negative electrode mixture is preferably 1% to 90% by mass, more preferably 10% to 70% by mass.
[0120] When a carbon material is mixed with a silicon-containing negative electrode active material and used as a negative electrode conductive agent, from the perspective of improving the cycle characteristics by enhancing the effect of electronic conductivity through mixing with the carbon material, the ratio of the silicon-containing negative electrode active material to the carbon material is based on the total net mass of silicon in the silicon-containing negative electrode active material in the negative electrode mixture, and the carbon material is preferably 10% by mass or more, more preferably 20% by mass or more. In addition, if the ratio of the carbon material mixed with the silicon-containing negative electrode active material is too large, the amount of silicon-containing negative electrode active material in the negative electrode mixture layer may be reduced, and the effect of increasing the capacity may be reduced. Based on the total mass of the carbon material, the net mass of silicon in the silicon-containing negative electrode active material is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more. In addition, it is more preferred that, if necessary, the conductive agent is compounded by premixing it with the silicon-containing active material and performing appropriate heat treatment.
[0121] When graphite is used, it is more preferred to use a carbon material having a graphite-type crystal structure, wherein the interplanar spacing (d002) of the graphite lattice plane (002) is 0.340 nm (nanometer) or less, particularly 0.335 nm to 0.337 nm. In particular, it is preferred to use artificial graphite particles having a block structure in which a plurality of flat graphite fine particles are assembled or bonded to each other in a non-parallel manner; or spherical particles of flaky natural graphite obtained by repeatedly applying mechanical actions (e.g., compression, friction, and shearing forces).
[0122] The ratio I(110) / I(004) is preferably 0.01 or more because the electrochemical characteristics in a wider temperature range can be improved, more preferably 0.05 or more, and even more preferably 0.1 or more, wherein I(110) / I(004) is a ratio of the peak intensity I(110) of the (110) plane of the graphite crystal to the peak intensity I(004) of the (004) plane, which is obtained by pressing the negative electrode into a shape having a density of 1.5 g / cm2 excluding the current collector. 3 The peak intensity ratio I(110) / I(004) is preferably less than 0.5, more preferably less than 0.3, because excessive treatment may reduce the crystallinity and discharge capacity of the battery.
[0123] In addition, it is preferred that the high crystalline carbon material (core material) is coated with a carbon material having a lower crystallinity than the core material, because the electrochemical properties in a wide temperature range can be further improved. The crystallinity of the coated carbon material can be confirmed by TEM. When a high crystalline carbon material is used, it reacts with a non-aqueous electrolyte during charging, and tends to deteriorate the characteristics of the lithium ion secondary battery in a wide temperature range (such as low temperature characteristics and gas generation after high temperature storage) due to an increase in interface resistance. However, if the polyimide adhesive precursor composition of the present invention is used, the characteristics of these lithium ion secondary batteries can be improved.
[0124] As the negative electrode mixture paste, the polyimide binder precursor composition of the present invention is used, and other binders may be used together, and the amount used is 95% by mass or less, and more preferably 45% by mass or less.
[0125] Examples of adhesives other than the polyimide adhesive precursor composition of the present invention include polyvinylidene fluoride, polytetrafluoroethylene, styrene butadiene rubber, butadiene rubber, nitrile rubber, polyacrylonitrile, ethylene-vinyl alcohol copolymer resin, ethylene propylene diene rubber, polyurethane, polyacrylic acid, polyamide, polyacrylate, polyvinyl ether, fluororubber, carboxymethyl cellulose and sodium carboxymethyl cellulose.
[0126] In addition, the electrode mixture paste of the present invention may further contain a solid electrolyte. Examples of the solid electrolyte include: oxide-based solid electrolytes, such as La having a perovskite crystal; 0.5 1Li 0.34 TiO 2.94 , Li7La3Zr2O with garnet crystals 12 , Li with NASICON-type crystal 1.3 Al 0.3 Ti 1.7 (PO4)3, amorphous LIPON (Li 2.9 PO 3.3 N 0.46 ); and sulfide solid electrolytes, such as Li2S-SiS2 materials and Li2S-P2S5 materials.
[0127] The electrode mixture paste of the present invention can be prepared into a uniform composition by applying the above-mentioned components to a known manufacturing method and by adding, stirring and mixing, etc. For example, the electrode mixture paste can be prepared by preparing a solution or dispersion in which a polyimide-based binder and a solvent are mixed, and then adding and mixing various additives.
[0128] <Negative electrode active material layer, negative electrode sheet>
[0129] The negative electrode mixture paste of the present invention is cast or coated on a conductive current collector, and then heated to remove the solvent, and optionally subjected to an imidization reaction, thereby forming a negative electrode (negative electrode sheet) having a negative electrode active material layer on the current collector. In the process of forming the negative electrode sheet, it is also preferred to use a roller press to press the negative electrode sheet until the desired electrode density is reached. Any known current collector can be used.
[0130] The polyimide precursor in the polyimide adhesive precursor composition is converted into a polyimide adhesive by heat treatment, and the particles of the active material and the conductive agent are combined with each other and with the current collector at the same time. The heat treatment can remove the solvent and imidize the polyimide precursor, thereby reducing the solubility in solvents such as electrolytes and improving solvent resistance. The heat treatment can be carried out at, for example, 80°C to 450°C. In order to promote imidization, it is preferred to heat so that the maximum temperature is preferably 180°C to 450°C, more preferably 200°C to 450°C, for example, 250°C to 380°C or above. In the temperature range below 200°C (or below 200°C), especially below 180°C (or below 180°C), the solvent is mainly removed. Therefore, the heat treatment can be divided into a step of mainly removing the solvent and a step of mainly carrying out imidization, that is, it can be carried out stepwise or continuously by dividing into step 1 of heating at 80° C. to 200° C. (or 180° C.) and step 2 of heating at a temperature of 200° C. or above (or 180° C. or above). In practice, imidization may be carried out in a high temperature range in step 1, and solvent removal may also occur in step 2 depending on the degree of solvent removal in step 1.
[0131] The time of steps 1 and 2 can be appropriately determined in consideration of the simplicity of the process, the desired imidization ratio, etc. The time of step 1 may be 0 seconds (when step 1 is not performed), but is preferably 1 minute or more, more preferably 10 minutes or more, and is preferably 5 hours or less, more preferably 2 hours or less, while the time of step 2 is preferably 10 minutes or more, more preferably 30 minutes or more, and is preferably 24 hours or less, more preferably 12 hours or less.
[0132] When the imidization rate of the polyimide precursor present in the polyimide adhesive precursor composition is high, for example, the imidization rate is 70% or more, preferably 80% or more (it may also be 90% or more or 100%), in some cases, only the above step 1 (mainly removing the solvent) may be sufficient as a heat treatment. However, in order to ensure the removal of the solvent and / or to increase the imidization rate, the above step 2 may also be performed.
[0133] The thickness of the negative electrode active material layer of the present invention can be appropriately determined according to the purpose and the required capacity. Although not limited, it is preferably used in the range of, for example, 0.1 μm to 500 μm. More preferably, it is 1 μm or more, even more preferably 10 μm or more, even more preferably 20 μm or more, and more preferably 300 μm or less, even more preferably 100 μm or less, even more preferably 50 μm or less.
[0134] <Positive Electrode Active Material>
[0135] As the positive electrode active material for lithium secondary batteries, a composite metal oxide containing at least one selected from cobalt, manganese, and nickel and lithium can be used. These positive electrode active materials can be used alone or in combination of two or more.
[0136] Examples of such lithium composite metal oxides include those selected from LiCoO2, LiMn2O4, LiNiO2, LiCo 1-x Ni x O2(0.01 <x<1)、LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2、LiNi 1 / 2 Mn 3 / 2 O4 and LiCo 0.98 Mg 0.02 Furthermore, these may be used in combination, such as LiCoO2 and LiMn2O4, LiCoO2 and LiNiO2, and LiMn2O4 and LiNiO2.
[0137] In addition, a part of the lithium composite metal oxide may be replaced with other elements to improve safety and cycle characteristics during overcharging, or to enable it to be used at a charging potential of 4.3 V or more. For example, a part of cobalt, manganese and nickel may be replaced with at least one or more elements such as Sn, Mg, Fe, Ti, Al, Zr, Cr, V, Ga, Zn, Cu, Bi, Mo and La. Alternatively, a part of O may be replaced with S or F, or a coating may be formed from a compound containing these other elements.
[0138] Among them, lithium composite metal oxides that can operate at a positive electrode charging potential of 4.3V or more relative to Li in a fully charged state are preferred, such as LiCoO2, LiMn2O4 and LiNiO2. More preferred are lithium composite metal oxides that can operate at a positive electrode charging potential of 4.4V or more, such as lithium cobalt oxides substituted with different elements, such as LiCo 1-x M xO2 (wherein M is one or more elements selected from Sn, Mg, Fe, Ti, Al, Zr, Cr, V, Ga, Zn and Cu, 0.001 ≤ x ≤ 0.05), and lithium composite metal oxides in which the ratio of nickel atoms and manganese atoms to all metal elements except lithium atoms is 50 atomic % or more and 100 atomic % or less, such as LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2、LiNi 0.5 Mn 0.3 Co 0.2 O2、LiNi 1 / 2 Mn 3 / 2 O4 and solid solutions of Li2MnO3 and LiMO2 (wherein M is a transition metal, such as Co, Ni, Mn, Fe, etc.). When using lithium composite metal oxides operating at high charging voltages, the characteristics of lithium ion secondary batteries tend to deteriorate when used in a wide temperature range due to reactions with electrolytes during charging. However, if the polyimide adhesive precursor composition of the present invention is used, the degradation of these lithium ion secondary battery characteristics can be suppressed.
[0139] In addition, as the positive electrode active material, a lithium-containing olivine phosphate can also be used. In particular, a lithium-containing olivine phosphate containing at least one selected from iron, cobalt, nickel and manganese is preferred. Specific preferred examples thereof include one or more selected from LiFePO4, LiCoPO4, LiNiPO4 and LiMnPO4.
[0140] Part of these lithium-containing olivine-type phosphates may be replaced with other elements, and part of iron, cobalt, nickel and manganese may be replaced with one or more elements selected from Co, Mn, Ni, Mg, Al, B, Ti, V, Nb, Cu, Zn, Mo, Ca, Sr, W and Zr, etc., or a coating may be formed from a compound or carbon material containing these other elements. Among them, LiFePO4 or LiMnPO4 is preferred.
[0141] Furthermore, the lithium-containing olivine-type phosphate may be used in a mixed manner with, for example, the above-mentioned positive electrode active material.
[0142] <Positive Electrode Conductive Agent>
[0143] There is no particular limitation on the positive electrode conductor, as long as it is a conductive material that does not cause chemical changes. Preferred examples thereof include: graphite, such as natural graphite (flaky graphite, etc.), artificial graphite and other graphites; one or more carbon blacks selected from acetylene black, Ketjen black, channel black, furnace black, lamp black and thermal black; and fibrous carbon powders, such as carbon nanotubes and carbon fibers. In addition, it is more preferred that the positive electrode conductor can be appropriately mixed and used in a mixture, such as graphite and carbon black, graphite and fibrous carbon powder, or carbon black and fibrous carbon powder. The amount of carbon material added to the positive electrode mixture is preferably 1% to 10% by mass, more preferably 2% to 5% by mass.
[0144] <Positive Electrode Binder>
[0145] As the positive electrode mixture slurry, the polyimide binder precursor composition of the present invention can be used, but other binders can also be used, examples of which include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), copolymers of styrene and butadiene (SBR), copolymers of acrylonitrile and butadiene (NBR), carboxymethyl cellulose (CMC) or ethylene propylene diene terpolymer.
[0146] Furthermore, the polyimide binder precursor composition of the present invention may be used in combination with other binders, but preferred embodiments thereof are the same as those described in the [Negative Electrode Binder] section.
[0147] <Positive electrode>
[0148] The positive electrode sheet is a sheet formed by casting or coating an electrode mixture paste which is a mixture of a positive electrode binder, a positive electrode active material, and optional components such as a conductive agent on a current collector to form an active material layer.
[0149] <Lithium-ion secondary battery>
[0150] The lithium ion secondary battery of one embodiment of the present invention includes the above-mentioned negative electrode (negative electrode sheet), and can adopt the known configuration required for the lithium ion secondary battery, such as the positive electrode (positive electrode sheet), the electrolyte and other required components (such as a separator). The lithium ion secondary battery can be a lithium polymer battery using a gel electrolyte as an electrolyte, or an all-solid-state battery using an inorganic solid electrolyte such as an oxide or sulfide electrolyte.
[0151] <Other power storage devices>
[0152] The polyimide binder of the present invention can be used not only for lithium ion secondary batteries but also for other power storage devices having a mechanism similar to that of lithium ion secondary batteries, such as lithium ion capacitors.
[0153] Example
[0154] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0155] The abbreviations of the compounds used in the following examples will be explained.
[0156] <Tetracarboxylic acid component>
[0157] H"-PMDA: Cyclohexane-1,2,4,5-tetracarboxylic dianhydride (chair isomer)
[0158] H'-PMDA: Cyclohexane-1,2,4,5-tetracarboxylic dianhydride (boat isomer)
[0159] CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride
[0160] CpODA: Norbornane-2-spiro-α-cyclopentanone-α'-spiro-2"-norbornane 5,5",6,6"-tetracarboxylic dianhydride
[0161] DNDAxx: (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethylnaphthalene-2t,3t,6c,7c-tetracarboxylic dianhydride
[0162] BTA: Bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride
[0163] H-sBPDA: [1,1'-bis(cyclohexane)]-3,3',4,4'-tetracarboxylic dianhydride
[0164] PPHT: (octahydro-1,3-dioxo-5-isobenzofurancarboxylic acid) 1,4-benzenediamide
[0165] PMDA: Pyromellitic Dianhydride
[0166] s-BPDA: 3,3',4,4'-biphenyltetracarboxylic dianhydride
[0167] [Diamine component]
[0168] ODA: 4,4'-diaminodiphenyl ether
[0169] PPD: p-phenylenediamine
[0170] TPE-R: 1,3-bis(4-aminophenoxy)benzene
[0171] BAPP: 2,2-bis[4-(4-aminophenoxy)phenyl]propane
[0172] MBAA: Bis(4-amino-3-carboxyphenyl)methane
[0173] DABAN: 4,4'-diaminobenzanilide
[0174] DATP: 4,4"-diaminoterphenyl
[0175] <Other>
[0176] EC: Ethylene carbonate
[0177] DEC: Diethyl carbonate
[0178] VC: Vinylene carbonate
[0179] NMP: N-methyl-2-pyrrolidone
[0180] Table 1
[0181]
[0182] <Calculation of Irreversible Capacity of Polyimide Adhesive>
[0183] (A1) Preparation of negative electrode for evaluation
[0184] Graphite (MAG-D; block artificial graphite, manufactured by Showa Denko Materials Co., Ltd., with an average particle size of 20 μm) as a negative electrode active material and a polyimide binder precursor composition (Examples and Comparative Examples) were mixed so that the solid ratios thereof were 92:8, 95:5 and 97:3 (mass %), and then NMP was added and mixed so that the slurry concentration became about 50 mass %, thereby preparing a negative electrode mixture paste.
[0185] The negative electrode mixture paste was coated on a nickel-plated steel foil (thickness 10 μm) as a current collector and pre-dried on a hot plate at 110°C for 3 minutes. Then, it was roll-pressed and placed in an electric furnace for heat treatment at 360°C for 1.5 hours under an argon flow to prepare a negative electrode for evaluation (2 mAh / cm 2 ).
[0186] (A2) Preparation of Evaluation Cells
[0187] Using the negative electrode for evaluation obtained in (1) above, a battery for evaluation having the following configuration was produced.
[0188] Cell shape: 2032 button cell
[0189] Counter electrode: lithium foil (metallic lithium)
[0190] Electrolyte: 1M LiPF6 / EC:DEC=1:1 (volume %) with 1% VC added
[0191] Diaphragm
[0192] (A3) Battery Evaluation
[0193] Charging and discharging were performed under the following conditions.
[0194] Measuring temperature: 30℃
[0195] Charge and discharge range: 0.001V to 2.0V
[0196] (However, the initial charge should be performed from the natural potential (about 3V) to 0.001V).
[0197] Charge and discharge current value: 0.02C
[0198] The charge capacity and discharge capacity (mAh / g) were calculated based on the weight of the entire active material layer (the sum of the active material weight and the binder weight). The difference between the first charge capacity and the first discharge capacity to 1 V was calculated as the irreversible capacity. Here, Li absorption in the "evaluation negative electrode" is referred to as "charge", and Li release in the "evaluation negative electrode" is referred to as discharge.
[0199] (A4) Calculation of the irreversible capacity of the polyimide adhesive itself
[0200] like Figure 1 As shown, the irreversible capacity of the battery calculated in (A3) above was plotted against the amount of polyimide binder added (mass %) to create a calibration curve. In the obtained calibration curve, the irreversible capacity when the binder addition amount was 100% was defined as the irreversible capacity of the polyimide itself.
[0201] <Evaluation of single-element silicon negative electrode using polyimide binder>
[0202] (B1) Preparation of single-element silicon negative electrode
[0203] Silicon (manufactured by Elkem, with an average particle size of 3 μm) as a negative electrode active material, a polyimide binder precursor composition (Examples and Comparative Examples) and a conductive aid (acetylene black, manufactured by DENKA) were mixed at a solid ratio of 60:30:10 (mass %) to prepare a negative electrode mixture paste. The negative electrode mixture paste was coated on a nickel-plated steel foil (thickness: 10 μm) as a current collector and pre-dried at 110° C. for 3 minutes. Then, it was rolled, placed in an electric furnace, and heat-treated at 360° C. for 1.5 hours under an argon gas flow to prepare a negative electrode (3 mAh / cm 2 ).
[0204] (B2) Evaluation of batteries using single-element silicon anodes
[0205] A battery was prepared in the same manner as in the above (A2), and charged and discharged under the following conditions.
[0206] Measuring temperature: 30℃
[0207] Charge and discharge range: 0.001V to 1.0V
[0208] (However, the initial charge should be performed from the natural potential (about 3V) to 0.001V).
[0209] Charge and discharge current value: 0.1C
[0210] (B3) Initial charge and discharge efficiency
[0211] The initial charge and discharge efficiency was calculated by the following formula.
[0212] Initial charge and discharge efficiency = (first discharge capacity to 1V) / (first charge capacity) × 100%
[0213] <Evaluation of Mechanical Properties of Polyimide Adhesive>
[0214] The polyimide adhesive precursor composition (Examples and Comparative Examples) was applied to a glass substrate using a spin coater, dried at 80°C for 10 minutes, and then heat-treated at 120°C for 30 minutes, at 150°C for 10 minutes, at 200°C for 10 minutes, at 250°C for 10 minutes, and at 350°C for 10 minutes in a nitrogen atmosphere (heating rate: 5°C / min) to obtain a film having a thickness of 10 μm. The obtained film was cut into strips having a width of 10 mm and a length of 200 mm to prepare test samples.
[0215] The test sample was mounted on a tensile testing machine with the clamp distance set to 100 mm, and the sample was stretched at a speed of 50 mm / min. The elastic modulus, elongation (elongation at break), and fracture energy were calculated based on the obtained stress-strain curve. The measurement environment was room temperature in the atmosphere.
[0216] <Production Examples and Comparative Examples of Polyimide Adhesive Precursor Compositions>
[0217] [Composition PI-1]
[0218] 160 g of NMP was added to the reaction container, and then the container was replaced with nitrogen and maintained at 50° C. 23.5916 g of ODA was added to the container and dissolved, and then a total of 26.3424 g of H”-PMDA (molar ratio to diamine was 1) and 40 g of NMP were gradually added, and the mixture was stirred overnight at 50° C. to obtain a polyimide adhesive precursor composition PI-1.
[0219] Viscosity 49P
[0220] [Compositions PI-2 to PI-12]
[0221] Polyimide adhesive precursor compositions PI-2 to PI-12 were obtained by reacting the tetracarboxylic dianhydride and diamine shown in Table 2 in the same manner as composition PI-1. The viscosity and concentration are shown in Table 2.
[0222] [Composition PI-10'] (Polyimide solution type composition)
[0223] A polyimide solution-type polyimide adhesive precursor composition is prepared by imidization from the same monomer composition as composition PI-10. First, 160 g of NMP is added to a reaction container, and the interior of the container is purged with nitrogen and maintained at 50°C. 32.3399 g of BAPP is added thereto and dissolved, and then the temperature of the reaction bath is raised to 70°C. A total of 17.6601 g of H"-PMDA (in a molar ratio of 1 to diamine) and 40 g of NMP are gradually added to the container. After stirring at 70°C for 30 minutes, the mixture is stirred at 170°C for 3 hours for imidization to obtain a polyimide adhesive precursor composition PI-10'. The viscosity and concentration are shown in Table 2.
[0224] [Compositions PI-13 to PI-14] (Copolymerized polyimide precursor)
[0225] Polyimide adhesive precursor compositions PI-13 and PI-14 were obtained by using two tetracarboxylic dianhydrides shown in Table 2 as tetracarboxylic acid components and using diamines shown in Table 2 and reacting them in the same manner as composition PI-1. The viscosity and concentration are shown in Table 2. For compositions using two or more compounds as tetracarboxylic acid components and diamine components, the molar ratio is shown in parentheses after the monomer.
[0226] [Compositions PI-15 to PI-18]
[0227] The tetracarboxylic dianhydride and diamine shown in Table 2 were reacted in the same manner as in composition PI-1 to obtain polyimide adhesive precursor compositions PI-15 to PI-18.
[0228] [Composition PI-MIX] (Polyimide Precursor Blend)
[0229] As shown in Table 2, two polyimide adhesive precursor compositions were mixed to obtain a polyimide adhesive precursor composition PI-MIX. The viscosity and concentration are shown in Table 2. In Table 2, the mixing ratio is shown in parentheses as a molar ratio (ratio of the total number of monomer units).
[0230] [Compositions PI-19 to PI-23]
[0231] Polyimide adhesive precursor compositions PI-19 to PI-23 were obtained by reacting the tetracarboxylic dianhydride and diamine shown in Table 2 in the same manner as composition PI-1. The viscosity and concentration are shown in Table 2.
[0232] Table 2
[0233]
[0234] <Evaluation Results of Polyimide Adhesive>
[0235] Using the prepared polyimide binder precursor composition, an evaluation battery was prepared according to <Calculation of Irreversible Capacity of Polyimide Binder>, and the battery was evaluated to prepare a calibration curve and calculate the irreversible capacity of the polyimide binder. The results are shown in Table 3.
[0236] <Evaluation of single-element silicon negative electrode using polyimide binder>
[0237] Using the prepared polyimide binder precursor composition, a negative electrode using silicon as a negative electrode active material was prepared according to <Evaluation of a single silicon negative electrode using a polyimide binder>. Then a battery was prepared and the initial charge and discharge efficiency was evaluated. The results are shown in Table 3.
[0238] Table 3
[0239]
[0240] It can be found from Table 3 that when the irreversible capacity of the polyimide binder is 1200 mAh / g or less, the initial charge and discharge efficiency of the battery using single silicon as the negative electrode active material is above 80%. Therefore, the use of the polyimide binder precursor composition of the present invention can increase the capacity of lithium ion secondary batteries.
[0241] <Evaluation Results of Mechanical Properties of Polyimide Adhesive>
[0242] The prepared polyimide adhesive precursor composition was used to measure the mechanical properties of the adhesive (elastic modulus, elongation (elongation at break) and breaking energy) according to <Evaluation of Mechanical Properties of Polyimide Adhesive>. The results are shown in Table 4. The results show that the polyimide adhesive obtained from the polyimide adhesive precursor composition of the present invention has excellent mechanical properties and can fully exert the function of the adhesive.
[0243] Table 4
[0244]
[0245] Industrial Applicability
[0246] The present invention can be suitably used as an electrode binder for power storage devices such as lithium ion secondary batteries.
Claims
1. A polyimide binder precursor composition for an electrode of a storage device, comprising a reaction product of a tetracarboxylic acid component and a diamine component and a solvent, in, The irreversible capacity of the polyimide adhesive obtained from the polyimide adhesive precursor composition is 1200 mAh / g or less.
2. The polyimide adhesive precursor composition according to claim 1, wherein The polyimide adhesive precursor composition includes a reaction product of a tetracarboxylic acid component containing 50 mol % or more of an alicyclic tetracarboxylic dianhydride and a diamine component, and a solvent.
3. The polyimide adhesive precursor composition according to claim 1, wherein The diamine component contains 50 mol % or more of an aromatic diamine compound. 4 . A negative electrode mixture paste for a power storage device, comprising the polyimide binder precursor composition according to claim 1 and an active material containing a silicon-containing material and / or graphite.
5. A negative electrode for an electric storage device, comprising: (a) an electrode active material layer, the electrode active material layer comprising an active material and a polyimide binder, the active material comprising a silicon-containing material and / or graphite, the polyimide binder being a heating product of a polyimide precursor in the polyimide binder precursor composition according to any one of claims 1 to 3; The polyimide binder binds the active material; as well as (b) Current collector. 6 . An electricity storage device comprising the negative electrode for an electricity storage device according to claim 5 .
7. A method for manufacturing a negative electrode for an electric storage device, comprising the following steps: Casting or coating the negative electrode mixture paste according to claim 4 on a current collector; and The coated layer of the negative electrode mixture paste is heated to form a negative electrode active material layer.
8. A method for manufacturing an electricity storage device, comprising the method for manufacturing a negative electrode according to claim 7 as a step.
Citation Information
Patent Citations
Binder for electrodes of lithium ion batteries, paste for negative electrodes of lithium ion batteries, and method for producing negative electrode of lithium ion battery
CN103238241A
Polyimide precursor and polyimide
CN105492496A
Polyimide binder for power storage device, electrode sheet using same, and power storage device
CN105580173A
Binder composition for secondary battery
CN110431696A
Resin composition, laminate and manufacturing method thereof, electrode, secondary battery, and electric double layer capacitor
CN110809607A