Current collector, electrode for electricity storage device, and lithium ion secondary battery
By using an aluminum metal layer supported by a resin layer in a lithium-ion secondary battery, optimizing the thickness and orientation of the aluminum metal layer solves the problem of insufficient resistance of the composite current collector in a non-aqueous electrolyte environment, and realizes lithium-ion High endurance and stability of secondary batteries.
Patent Information
- Application Number
- CN202280092922.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-02
- Publication Date
- 2024-10-29
AI Technical Summary
Existing composite current collectors have insufficient resistance to non-aqueous electrolyte environments, and are prone to deterioration especially under high temperature conditions, resulting in reduced charge and discharge characteristics of lithium-ion secondary batteries.
An aluminum metal layer supported by a resin layer is used as the current collector. By optimizing the thickness and orientation of the aluminum metal layer in the X-ray diffraction method, a highly dense conductive layer is formed to improve the resistance to non-aqueous electrolytes.
The resistance of the current collector is significantly improved, the peeling of the conductive layer is suppressed, and the charge and discharge characteristics and reliability of the lithium-ion secondary battery are maintained.
Smart Images

Figure CN118872099A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a current collector, an electrode for a power storage device, and a lithium ion secondary battery. Background Art
[0002] As a current collector for a secondary battery, it has been proposed to use a composite material having a conductive layer formed on one or both surfaces of a resin film. Patent Document 1 discloses a secondary battery using such a composite material as a current collector.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: U.S. Patent Application Publication No. 2020 / 0373584 Summary of the invention
[0006] Technical problem to be solved by the invention
[0007] When the current collector of the composite material is used in a storage device such as a lithium ion secondary battery having a non-aqueous electrolyte, the current collector preferably has resistance to the non-aqueous electrolyte. One embodiment of the present disclosure provides a current collector having excellent resistance to the non-aqueous electrolyte, an electrode for a storage device, and a lithium ion secondary battery.
[0008] Means for solving technical problems
[0009] A collector according to one embodiment of the present disclosure comprises: a resin layer having a first surface and a second surface located on the opposite side of the first surface; and a first metal layer located on the first surface, wherein the first metal layer contains aluminum as a main component, and a thickness d of the first metal layer is not less than 0.5 μm and not more than 3 μm. In a measurement of the first metal layer based on an X-ray diffraction method, when a peak intensity ratio B / A of an intensity A of a highest X-ray diffraction peak in a range of a diffraction angle (2θ) of not less than 36° and not more than 41° and an intensity B of a highest X-ray diffraction peak in a range of a diffraction angle (2θ) of not less than 43° and not more than 48° is set to r, d and r satisfy the following formula (1),
[0010]
[0011] Effects of the Invention
[0012] According to one embodiment of the present disclosure, a current collector, an electrode for a power storage device, and a lithium ion secondary battery having excellent resistance to a non-aqueous electrolyte solution can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 This is a schematic cross-sectional view showing an example of the current collector according to the first embodiment.
[0014] Figure 2 An example of an X-ray diffraction pattern of an aluminum thin film is shown.
[0015] Figure 3 This is a schematic cross-sectional view showing an example of a current collector according to the second embodiment.
[0016] Figure 4 It is a schematic exploded perspective view showing an example of the electricity storage device electrode according to the third embodiment.
[0017] Figure 5 This is a schematic partially cutaway perspective view showing an example of a lithium ion secondary battery according to a fourth embodiment.
[0018] Figure 6 Yes means Figure 5 FIG. 1 is a schematic exploded perspective view of an example of a battery cell (Cell) of a lithium-ion secondary battery shown in FIG.
[0019] Figure 7 The X-ray diffraction patterns obtained from the samples of Examples 2, 5, and 7 show the range of diffraction angles (2θ) of 43° to 48° where the peak of Al (200) can be observed.
[0020] Description of Reference Numerals
[0021] 10 resin layer
[0022] 10a Side 1
[0023] 10b Side 2
[0024] 20First metal layer
[0025] 20' Second metal layer
[0026] 101, 102, 210 collector
[0027] 201, 201'Electrodes for power storage devices
[0028] 210 collector
[0029] 210s Part 1
[0030] 210t Part 2
[0031] 220 active material layer
[0032] 301 lithium ion secondary battery
[0033] 310 battery cell
[0034] 311 lead wire
[0035] 313 outer body
[0036] 314 Electrolyte
[0037] 320 Diaphragm DETAILED DESCRIPTION
[0038] The current collector having a conductive layer formed on a resin film is different from the metal foil used as a current collector in terms of structure and thickness. In particular, the conductive layer is supported by the resin film and is thinner than the metal foil used in the existing current collector.
[0039] Lithium-ion secondary batteries usually have a non-aqueous electrolyte containing anions containing fluorine atoms as electrolytes. When the above-mentioned current collector is used in a lithium-ion secondary battery, the current collector needs to have appropriate resistance to the non-aqueous electrolyte. For example, when such a lithium-ion secondary battery is charged and discharged in a high-temperature environment, the anions containing fluorine atoms decompose, and fluoride ions, i.e., hydrofluoric acid, are generated as decomposition products. The inventors of the present application have come up with the idea of suppressing the deterioration of the current collector on which a conductive layer is formed on a resin film by suppressing the decomposition products of the non-aqueous electrolyte, specifically suppressing the peeling of the conductive layer from the resin film, thereby suppressing the deterioration of the current collector and maintaining the charge and discharge characteristics of the current collector, the electrode for a storage device, and a lithium-ion secondary battery.
[0040] Below, while referring to the attached Figure 1 The embodiments of the collector, the electrode for the storage device, and the lithium-ion secondary battery disclosed in the present invention are described. The numerical values, shapes, materials, steps, and the order of the steps mentioned in the following description are only examples, and various changes can be made as long as there is no technical contradiction. In addition, the embodiments described below are also only examples, and various combinations can be made as long as there is no technical contradiction.
[0041] The thickness, size, shape, etc. of the components shown in the drawings of the present disclosure are sometimes exaggerated for the sake of convenience. In addition, in the drawings of the present disclosure, in order to avoid excessive complexity, a part of the components are sometimes taken out for illustration, or the illustration of a part of the elements is omitted. Therefore, the size of each component and the configuration between components shown in the drawings of the present disclosure sometimes do not reflect the size of each component and the configuration between components in the actual device. The "vertical" and "orthogonal" of the present disclosure are not limited to two straight lines, edges, surfaces, etc. strictly forming an angle of 90°, but include situations within the range of 90°±5°. In addition, "parallel" includes situations where two straight lines, edges, surfaces, etc. are within the range of 0°±5°.
[0042] In this specification, the term "battery cell" refers to a structure in which at least one pair of positive and negative electrodes are integrally assembled. The term "battery" in this specification is used as a term including various forms such as a battery module, a battery pack, etc. having one or more "battery cells" electrically connected to each other.
[0043] (First Embodiment)
[0044] Figure 1 : is a schematic cross-sectional view showing an example of the current collector of the present embodiment. The current collector of the present embodiment can also be used as a current collector for either the positive electrode or the negative electrode of a power storage device such as a lithium ion secondary battery. Figure 1 The current collector 101 shown includes a resin layer 10 having a first surface 10 a and a second surface 10 b located on the opposite side to the first surface 10 a , and a first metal layer 20 .
[0045] The resin layer 10 functions as a support for the first metal layer 20 in the current collector 101. The resin layer 10 has a lower density than the first metal layer 20, and thus can contribute to an increase in charge capacity per unit weight when the current collector 101 is applied to an electricity storage device.
[0046] The resin layer 10 has electrical insulation properties and contains resin. The resin layer 10 may also have thermoplastic properties. The resin layer 10 may contain at least one selected from polyethylene terephthalate (PET), polypropylene (PP), polyamide (PA), polyimide (PI), polyethylene (PE), polystyrene (PS), phenolic resin (PF) and epoxy resin (EP). The resin layer 10 may be a single layer or may be composed of a plurality of layers stacked together. In this case, at least one of the plurality of layers may contain a resin different from that of the other layers.
[0047] The thickness of the resin layer 10 is, for example, not less than 3 μm and not more than 12 μm. The thickness of the resin layer 10 may also be not less than 3 μm and not more than 6 μm. By having a thickness of the resin layer 10 of not less than 3 μm, sufficient strength as a support can be obtained. In addition, by having a thickness of the resin layer 10 of not more than 12 μm, the overall thickness of the collector 101 can be reduced. Therefore, in a stacked lithium-ion secondary battery having a plurality of electrode pairs stacked therein, the proportion of the portion that does not contribute to energy accumulation, i.e., the current collector, can be reduced, and the energy density can be increased. If the thickness of the resin layer 10 is not more than 6 μm, the overall thickness of the collector 101 can be further reduced, and the energy density of the stacked lithium-ion secondary battery can be increased.
[0048] The current collector 101 may further include an undercoat layer between the resin layer 10 and the first metal layer 20. The undercoat layer may be provided to improve the bonding strength between the resin layer 10 and the first metal layer 20, or to suppress the formation of pinholes on the first metal layer 20. The undercoat layer may also be a layer formed of an organic material such as an acrylic resin or a polyolefin resin, or a layer containing a metal formed by sputtering.
[0049] The first metal layer 20 contains Al (aluminum) as a main component. Here, the main component refers to the element with the largest proportion of the constituent elements expressed in molar percentage when the component contains one or more constituent elements. If Al is contained as the main component, the first metal layer 20 may also contain other metals.
[0050] The thickness d of the first metal layer 20 is, for example, not less than 0.5 μm and not more than 3 μm. By setting the thickness d of the first metal layer 20 to be not less than 0.5 μm, the resistance of the first metal layer 20 can be reduced. For example, in the case of manufacturing a storage device, the energy loss caused by the resistance in the collector can be reduced. In addition, by setting the thickness of the first metal layer 20 to be not more than 3 μm, it is easy to obtain advantages such as a smaller proportion of the first metal layer 20 in the entire collector 101 and the use of the resin layer 10 to reduce the weight of the collector. The thickness d of the first metal layer 20 can also be not less than 0.7 μm and not more than 2 μm.
[0051] In the measurement based on the X-ray diffraction method, the first metal layer 20 has strong peaks in the range of diffraction angle (2θ) of 36° to 41° and in the range of diffraction angle (2θ) of 43° to 48°. Here, the highest X-ray diffraction peak in the range of diffraction angle (2θ) of 36° to 41° is the peak of Al (111), and the highest X-ray diffraction peak in the range of diffraction angle (2θ) of 43° to 48° is the peak of Al (200). The measurement based on the X-ray diffraction method is based on the Out of Plane method. That is, X-rays are incident from the surface of the first metal layer 20, and the intensity of the scattered X-rays is measured.
[0052] Figure 2 An example of X-ray diffraction peaks of aluminum thin film. Figure 2 As shown in FIG. 1 , a peak of the (111) plane is observed in the range of 36° to 41°, and a peak of the (200) plane is observed in the range of 43° to 48°. Aluminum metal has an fcc structure, and therefore, according to the extinction rule, peaks are observed only when the values of h, k, and l when the Miller indices are recorded as (h, k, and l) are all even numbers or all odd numbers.
[0053] When the peak intensity ratio B / A of the intensity A of the highest X-ray diffraction peak using the diffraction angle (2θ) in the range of 36° to 41° to the intensity B of the highest X-ray diffraction peak in the range of 43° to 48° is set to r, d and r of the first metal layer 20 satisfy the following formula (1):
[0054]
[0055] As described in detail in the following examples, when r and d satisfy the formula (1), the first metal layer 20 has excellent resistance to the non-aqueous electrolyte.
[0056] More preferably, d and r of the first metal layer 20 satisfy the following formula (2):
[0057]
[0058] As a result, the volume resistivity of the first metal layer 20 is reduced, and a low-resistance current collector is obtained.
[0059] In the formulas (1) and (2), d is a value when the thickness of the first metal layer is expressed in units of μm. The value of the thickness d of the first metal layer 20 is obtained by, for example, cross-sectional observation using SEM.
[0060] Preferably, r satisfies the following formula (3):
[0061] r<1 (3).
[0062] When r satisfies the formula (3), the (111) orientation of the first metal layer 20 becomes higher, and a denser metal layer can be obtained. Therefore, the resistance of the first metal layer 20 to the non-aqueous electrolyte is further improved.
[0063] It is more preferable that the peak of Al(200) is hardly observed. That is, it is preferable that the peak intensity B of Al(200) is of the same degree as the intensity of the baseline in the measurement based on the X-ray diffraction method. The same degree means that there is actually no difference in the intensity unevenness caused by noise from the baseline in the measurement based on the X-ray diffraction method. When the peak intensity B of Al(200) is of the same degree as the intensity of the baseline in the measurement based on the X-ray diffraction method, it can be regarded as B=0. Therefore, in this case, The value of may also be equal to 0. If, on the other hand, the peak intensity B of Al(200) is large enough to be distinguished from the noise of the baseline in the measurement based on the X-ray diffraction method, then Use a value greater than 0.
[0064] The orientation index of the (111) plane of aluminum in the first metal layer in the direction perpendicular to the first surface 10a of the resin layer 10 based on the Lotgering method is preferably 0.8 or more. This increases the (111) orientation of the first metal layer 20 and enables a denser metal layer to be obtained.
[0065] Here, the orientation index of the (111) plane refers to the orientation index F based on the Lotgering method. The maximum value of the orientation index based on the Lotgering method is 1. When the orientation index is 1, it means complete orientation, and when the orientation index is 0, it means no orientation. The orientation index F is calculated by the following formula using the intensity of the X-ray diffraction peak obtained by X-ray diffraction measurement of the layer (film) to be evaluated.
[0066]
[0067] I0(111) represents the intensity of the X-ray diffraction peak of the (111) plane obtained by X-ray diffraction measurement of a non-oriented Al film. I0(hkl) represents the intensity of the total diffraction peak obtained by X-ray diffraction measurement of a non-oriented Al film. In addition, a non-oriented Al film refers to an Al film that exhibits an intensity pattern of an X-ray diffraction peak that is close to the intensity pattern of an X-ray diffraction peak in a standard sample of aluminum disclosed in JCPDS (Joint Committee on Powder Diffraction Standards).
[0068] I(111) represents the intensity of the X-ray diffraction peak of the (111) plane obtained by X-ray diffraction measurement of the layer (film) to be evaluated. I(hkl) represents the intensity of the total diffraction peak obtained by X-ray diffraction measurement of the layer (film) to be evaluated.
[0069] In addition, the orientation index F based on the Lotgering method sometimes becomes a negative value. This negative value may occur when the intensity of the X-ray diffraction peak on the orientation plane from which the orientation index F is obtained from the layer (film) to be evaluated is smaller than the intensity obtained from the non-oriented film. When the orientation index F obtained by the above formula becomes a negative value, for example, the layer to be evaluated may be strongly oriented in an orientation direction other than the orientation plane from which the orientation index F is obtained.
[0070] The first metal layer 20 can be formed by any method as long as it has the above-mentioned characteristics. The first metal layer 20 can be formed on the resin layer 10 by a thin film forming technique such as sputtering or vacuum evaporation. In this case, by changing the film forming time, the vacuum degree reached during film forming, the film forming speed, the heating temperature of the substrate, the bias voltage and other conditions, the thickness of the first metal layer 20, the peak intensity of Al(111) and the peak intensity of Al(200) in the first metal layer 20 can be adjusted.
[0071] According to the present embodiment, the first metal layer 20 satisfies the above formula (1), so that the current collector 101 exhibits excellent electrolyte resistance. Therefore, the lithium ion secondary battery including the current collector 101 of the present embodiment suppresses degradation of battery characteristics and has excellent reliability.
[0072] (Second Embodiment)
[0073] Figure 3 1 is a schematic cross-sectional view showing an example of a current collector according to the present embodiment. The current collector 102 according to the present embodiment is different from the current collector 101 according to the first embodiment in that conductive layers are provided on both surfaces of the resin layer 10 .
[0074] The current collector 102 includes the resin layer 10 , the first metal layer 20 , and the second metal layer 20 ′. As described in the first embodiment, the first metal layer 20 is disposed on the first surface 10 a. On the other hand, the second metal layer 20 ′ is disposed on the second surface 10 b of the resin layer 10 .
[0075] Similar to the first metal layer 20, the second metal layer 20' also contains aluminum as a main component. The thickness d' of the second metal layer 20' is preferably not less than 0.5 μm and not more than 3 μm. In the measurement of the second metal layer 20' based on the X-ray diffraction method, when the peak intensity ratio B' / A' of the intensity A' of the highest X-ray diffraction peak in the range of the diffraction angle (2θ) of not less than 36° and not more than 41° and the intensity B' of the highest X-ray diffraction peak in the range of the diffraction angle (2θ) of not less than 43° and not more than 48° is set to r', d' and r' satisfy the following formula (4),
[0076]
[0077] Therefore, the second metal layer 20 ′ also has excellent resistance to non-aqueous electrolyte solutions.
[0078] More preferably, d' and r' of the second metal layer 20' satisfy the following formula (5):
[0079]
[0080] This reduces the volume resistivity of the second metal layer 20 ′, and a low-resistance current collector can be obtained.
[0081] Preferably, r' satisfies the following formula (6):
[0082] r'<1 (6).
[0083] By satisfying the formula (6), the (111) orientation of the second metal layer 20' becomes higher, and a denser metal layer can be obtained.
[0084] The orientation index of the aluminum (111) plane in the second metal layer 20' in the direction perpendicular to the second surface 10b of the resin layer 10 based on the Lotgering method is preferably 0.8 or more. This increases the (111) orientation of the second metal layer 20' and enables a denser metal layer to be obtained.
[0085] According to the current collector 102, the first metal layer 20 is provided on the first surface 10a of the resin layer 10, and the second metal layer 20' is provided on the second surface 10b, so that electrodes can be formed on both surfaces of the current collector 102. Therefore, the proportion of the resin layer in the power storage device can be reduced, and the battery capacity per unit area can be increased.
[0086] (Third Embodiment)
[0087] An embodiment of an electrode for a power storage device will be described. The electrode for a power storage device of this embodiment can be used for either a positive electrode or a negative electrode of a power storage device. Figure 4 : This is an exploded perspective view of an electrode 201 for an electrical storage device. The electrode 201 for an electrical storage device includes a current collector 210 and an active material layer 220. The current collector 210 includes a first portion 210s and a second portion 210t, and the active material layer 220 is arranged in the first portion 210s. The active material layer 220 is not provided in the second portion 210t, and the second portion 210t functions as a tab for electrical connection to the outside. The active material layer 220 may include an active material that is oxidized and reduced with charging (or storage) and discharging. The current collector 210 supports the active material layer 220, supplies electrons to the active material layer 220, and receives electrons from the active material layer 220.
[0088] The current collector 210 may be the current collector 101 or the current collector 102 described in the first embodiment or the second embodiment. Figure 4 The other active material layer not shown is arranged on the first portion 210 s on the back side (the side where the active material layer 220 is not arranged) of the current collector 210 .
[0089] The active material layer 220 may include a positive electrode active material or a negative electrode active material that absorbs and releases lithium ions. The positive electrode active material, for example, includes a composite metal oxide containing lithium. As composite metal oxides containing lithium, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), lithium manganese spinel (LiMn2O4), lithium vanadium compound (LiV2O5), olivine-type LiMPO4 (wherein M is one or more elements or vanadium oxides selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr), lithium titanate (Li4Ti5O 12 ), with the general formula: LiNi x Co y Mn z M a O2 (x+y+z+a=1, 0≤x<1, 0≤y<1, 0≤z<1, 0≤a<1, M in the above general formula is one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, Cr) represented by a composite metal oxide, and a general formula: LiNi x Co y Al z A composite metal oxide represented by O2 (0.9<x+y+z<1.1), etc. The positive electrode active material may contain polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene, etc. as a material capable of absorbing and releasing lithium ions.
[0090] The active material layer 220 may also include at least one of a binder and a conductive aid. The binder can use various known materials. When using the storage device electrode 201 as the positive electrode, as the binder in the active material layer 220, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), polytrifluorochloroethylene (PCTFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE) and polyvinyl fluoride (PVF) and other fluororesins can be used.
[0091] As the binder, vinylidene fluoride-based fluororubber may also be used. For example, vinylidene fluoride-hexafluoropropylene-based fluororubber (VDF-HFP-based fluororubber), vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene-based fluororubber (VDF-HFP-TFE-based fluororubber), vinylidene fluoride-pentafluoropropylene-based fluororubber (VDF-PFP-based fluororubber), vinylidene fluoride-pentafluoropropylene-tetrafluoroethylene-based fluororubber (VDF-PFP-TFE-based fluororubber), vinylidene fluoride-perfluoromethyl vinyl ether-tetrafluoroethylene-based fluororubber (VDF-PFMVE-TFE-based fluororubber), vinylidene fluoride-chlorotrifluoroethylene-based fluororubber (VDF-CTFE-based fluororubber), etc. may also be used as the binder of the active material layer 220.
[0092] Examples of the conductive additive include carbon materials such as carbon powder and carbon nanotubes. Carbon powder can be carbon black or the like. When the storage device electrode 201 is used as a positive electrode, another example of the conductive additive of the active material layer 220 is metal powder such as nickel, stainless steel, iron, and powder of conductive oxides such as ITO. Two or more of the above materials may be mixed and contained in the active material layer 220.
[0093] The negative electrode active material may include a carbon material. Examples of carbon materials include natural or artificial graphite, carbon nanotubes, non-graphitizable carbon, easily graphitizable carbon (soft carbon), and low-temperature sintered carbon. The negative electrode active material may also include materials other than carbon materials. For example, it may include alkali metals and alkaline earth metals such as metallic lithium, metals such as tin that can form compounds with metals such as lithium, or silicon, silicon-carbon composite materials, and amorphous compounds (SiO x (0<x<2), tin dioxide, etc.), lithium titanate (Li4Ti5O 12 ) and other particles.
[0094] When the storage device electrode 201 is used as a negative electrode, the above-mentioned binder and conductive aid can be used as the binder and conductive aid of the active material layer 220. In addition, as the binder for the negative electrode, cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide, polyamide-imide, acrylic resin, etc. can also be used.
[0095] The positive electrode and the negative electrode of the storage device electrode can be manufactured by a known manufacturing method. In the storage device electrode of the present embodiment, the adhesion between the resin layer and the conductive layer of the collector is improved. Therefore, the lithium ion secondary battery including the storage device electrode of the present embodiment can suppress the peeling of the conductive layer from the resin layer even under conditions where the electrolyte is easily decomposed, such as when used at high temperature, and can suppress the reduction of battery characteristics caused by the deterioration of the collector.
[0096] (Fourth Embodiment)
[0097] An embodiment of a lithium ion secondary battery will be described. Figure 5 is a schematic external view showing an example of a lithium ion secondary battery. Figure 6 Yes Figure 5 An exploded perspective view showing a battery cell in a lithium-ion secondary battery shown. Here, as a lithium-ion secondary battery, a pouch-type or laminated lithium-ion secondary battery is exemplified. The lithium-ion secondary battery shown is a single-layer type, but may also be a laminated type. In the example shown, the positive electrode, separator, and negative electrode constituting the battery cell are laminated along the Z direction of the figure.
[0098] Figure 5 The lithium ion secondary battery 301 shown includes a battery cell 310 , a pair of leads 311 connected to the battery cell 310 , an exterior body 313 covering the battery cell 310 , and an electrolyte 314 .
[0099] like Figure 6 Schematically shown in FIG. 1 , the battery cell 310 includes an electricity storage device electrode 201, an electricity storage device electrode 201', and a separator 320 disposed therebetween. In the example shown in the figure, the battery cell 310 is a single-layer battery cell including a pair of electrodes.
[0100] The same structure as that of the storage device electrode described in the third embodiment can be applied to each of the storage device electrode 201 and the storage device electrode 201'. In this example, one of the storage device electrode 201 and the storage device electrode 201' is configured as a positive electrode including a positive electrode active material, and the other is configured as a negative electrode including a negative electrode active material.
[0101] The separator 320 is an insulating porous material. For example, a single-layer film or a laminated film selected from polyolefins such as polyethylene and polypropylene, or a non-woven fabric or a porous film of at least one fiber selected from cellulose, polyester, polyacrylonitrile, polyimide, polyamide (such as aromatic polyamide), polyethylene and polypropylene can be used for the separator 320.
[0102] Electrolyte 314 is also arranged in the space inside outer casing 313. Electrolyte 314 is a non-aqueous electrolyte containing lithium ions, for example, a non-aqueous electrolyte solution containing lithium ions. When a non-aqueous electrolyte solution is used as electrolyte 314, a sealing material (for example, a resin film such as polypropylene, etc.) is typically arranged between outer casing 313 and lead 311 to prevent leakage of the non-aqueous electrolyte solution. Figure 5 (not shown in the figure).
[0103] As the electrolyte 314, for example, a non-aqueous electrolyte containing a metal salt such as a lithium salt and an organic solvent can be used. Examples of the lithium salt include LiPF6, LiClO4, LiBF4, LiCF3SO3, LiCF3CF2SO3, LiC(CF3SO2)3, LiN(CF3SO2)2, LiN(CF3CF2SO2)2, LiN(CF3SO2)(C4F9SO2), LiN(CF3CF2CO)2, and LiBOB. One of these lithium salts may be used alone, or two or more may be mixed and used.
[0104] For example, cyclic carbonate and chain carbonate can be used as the solvent of the electrolyte 314. Examples of the solvent of the electrolyte 314 include ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, and the like.
[0105] The lithium ion secondary battery 301 can be manufactured, for example, by the following method. First, the storage device electrodes 201 and 201' are prepared as described in the above embodiment. Then, the storage device electrodes 201 and 201' are held in a manner such that the active material layers are opposite to each other via the separator 320, and these components are inserted into the space of the outer casing 313. The electrolyte 314 is arranged in the space of the outer casing 313 and the outer casing 313 is sealed, thereby completing the lithium ion secondary battery 301.
[0106] According to the lithium ion secondary battery 301, the adhesion between the resin layer and the conductive layer of the current collector is improved. Therefore, even when the lithium ion secondary battery is used at high temperature, the conductive layer is further prevented from peeling off from the resin layer, and the reduction in battery characteristics caused by the deterioration of the current collector is suppressed.
[0107] (Example)
[0108] Current collectors of Examples and current collectors of Reference Examples were produced, and their characteristics were evaluated.
[0109] [Preparation of samples]
[0110] The current collectors of Examples 1 to 15 and Reference Examples 1 to 8 were prepared by the following method. Table 1 shows the formation conditions of the first metal layer of the current collectors of Reference Examples 1 to 8 and Examples 1 to 15.
[0111] Example 1 to Example 15
[0112] Production Figure 3The collector 102 of the structure shown. The resin layer 10 uses a polyethylene terephthalate resin with a thickness of 6 μm. The first metal layer 20 and the second metal layer 20' are formed by vacuum evaporation of Al. The thickness of each of the first metal layer 20 and the second metal layer 20' is adjusted by the film forming time. In order to produce samples in various crystalline states, as shown in Table 1, the vacuum degree reached and the film forming speed when forming these metal layers are different among these collectors. Table 1 shows the true pressure reached and the film forming speed when forming the first metal layer 20 of the collectors of Examples 1 to 15. The classification of the reaching pressure and film forming speed shown in Table 1 is shown in Tables 2 and 3.
[0113] Reference Example 1 to Reference Example 8
[0114] The current collectors of Reference Examples 1 to 8 were prepared in the same order as in Examples 1 to 15. Table 1 shows the reaching pressure and film forming speed when forming the first metal layer 20 of the current collectors of Reference Examples 1 to 8. The reaching pressure and film forming speed shown in Table 1 are classified as shown in Tables 2 and 3.
[0115] [evaluate]
[0116] (1) Thickness of the first metal layer
[0117] The thickness d of the first metal layer 20 in Examples 1 to 15 and Reference Examples 1 to 8 was determined by SEM observation of a cut surface of each current collector.
[0118] (2) Measurement based on X-ray diffraction
[0119] The crystallinity of the first metal layer 20 in each of the current collectors of Examples 1 to 15 and Reference Examples 1 to 8 was evaluated by X-ray diffraction.
[0120] The apparatus and measurement conditions used in the measurement are as follows.
[0121] Device name: PAN alytical X'Pert PRO, manufactured by Malvern Panalytical Ltd
[0122] Accelerating voltage: 45 kV
[0123] Current: 40mA
[0124] Scanning speed: 7deg. / min.
[0125] Sampling width: 0.008deg.
[0126] Based on the obtained X-ray diffraction pattern, the peak intensity A of Al(111) and the peak intensity B of Al(200) were determined for each sample, and the value of r=B / A was calculated. In addition, the Lotgering factor of Al(111) was obtained based on the peak intensity A of Al(111).
[0127] (3) Surface resistance
[0128] The surface resistance of the first metal layer 20 in each current collector of Examples 1 to 15 and Reference Examples 1 to 8 was measured using a four-terminal measurement device (manufactured by Nittoseiko Analytech Co., Ltd., LORESTA AX MCP-T370). Based on the value of the surface resistance of the first metal layer 20 and the thickness d, the volume resistivity of the first metal layer 20 of each sample was determined.
[0129] (4) Electrolyte resistance
[0130] The current collectors of Examples 1 to 15 and Reference Examples 1 to 8 were maintained in an environment similar to that of a lithium-ion secondary battery, and the presence or absence of peeling of the conductive layer was evaluated. Specifically, a non-aqueous electrolyte containing dimethyl carbonate of LiPF6 at a concentration of 1 mol% was prepared, and water was added to the non-aqueous electrolyte at a ratio of 1000 mass ppm and poured into a container. The prepared current collector was immersed in the non-aqueous electrolyte in the container, the whole was sealed with a laminated film, and stored in a thermostatic bath at 85°C for 72 hours (high temperature storage). Then, the current collector was removed from the laminated film and washed with an organic solvent.
[0131] The electrolyte resistance is evaluated for the current collector obtained after high temperature storage. The electrolyte resistance is evaluated by the following method. The surface of the conductive layer of the current collector after high temperature storage is wiped with a cotton swab. If a part of the conductive layer adheres to the cotton swab, it is determined that the conductive layer is peeled off from the resin layer and is judged as not possible (POOR). If the peeling of the conductive layer caused by the friction using the cotton swab is not confirmed, it is judged as good (GOOD).
[0132] Table 1 shows the evaluation results.
[0133]
[0134] [Table 2]
[0135] The ultimate pressure P(Pa) Classification <![CDATA[6×10 -2 <P]]> high <![CDATA[3×10 -2 <P≤6×10 -2 ]]> middle <![CDATA[1×10 -2 <P≤3×10 -2 ]]> Low <![CDATA[P≤1×10 -2 ]]> Very low
[0136] [Table 3]
[0137] Film forming speed R (μm·m / min) Classification 8<P high 4<P≤8 middle 0<P≤4 Low
[0138] [Results and Investigation]
[0139] As shown in Table 1, in the current collectors of Examples 1 to 15 and Reference Examples 1 to 8, d, r, The range is 0.33≤d≤2.00, 0.01≤r≤21.4, When r and d satisfy the relationship of formula (1), that is, When the value of is 2.1 or less, the electrolyte resistance is good (GOOD) in the current collector of any sample except Reference Example 2. When the value of is greater than 2.1, the electrolyte resistance is poor (POOR). The reason why the electrolyte resistance of the current collector of Reference Example 2 is poor is considered to be that the thickness d of the first metal layer 20 is less than 0.5 μm.
[0140] It can be seen that the volume resistivity of the first metal layer 20 in Examples 1 to 15 is in the range of 3.6 to 5.2 μΩ·cm. On the other hand, when r and d satisfy the relationship of formula (2), that is, When the value of is 1 or less, the volume resistivity of the first metal layer 20 is in the range of 3.6 to 4.52 μΩ·cm, and the first metal layer 20 with lower resistance can be obtained.
[0141] In the samples where the Lotgering factor of Al(111) is negative, the intensity B of the peak of Al(200) is greater than the intensity A of the peak of Al(111) except for Example 11. It is considered that the peak intensity A of Al(111) and the peak intensity B of Al(200) are in a trade-off relationship. Figure 7 The figure shows the range of diffraction angles (2θ) of 43° to 48° where the peak of Al(200) is observed in the X-ray diffraction patterns obtained from the samples of Examples 2, 5, and 7. The peak intensity A of Al(111) decreases in the order of Example 2, Example 7, and Example 5, while the peak intensity B of Al(200) increases in the order of Example 2, Example 7, and Example 5. In Example 2, the peak of Al(200) is not observed in the range of 43° to 48°, and the peak intensity of Al(200) is about the same as the intensity of the baseline of the X-ray diffraction pattern. That is, in the data of Example 2, it can be said that the peak intensity B is actually 0.
[0142] If the results of the collectors of Examples 5 and 6, and the collectors of Examples 11 and 12, in which the thickness of the first metal layer 20 is approximately the same, are compared, the value of the volume resistivity of the sample in which the peak intensity A of Al(111) is larger than the peak intensity B of Al(200) becomes smaller. It is believed that this is the result of the increase in the orientation of Al(111), thereby reducing the voids in the first metal layer 20, and the increase in density, thereby reducing the volume resistivity. It is believed that even if the intensity B of the peak of Al(200) increases, that is, the orientation of Al(200) increases, and the voids in the first metal layer 20 also decrease, it is believed that according to the embodiment, the peak intensity A of Al(111) is likely to show a larger value than that of Al(200), that is, it is easy to obtain an Al film with a (111) orientation having high crystallinity, and it is easy to reduce the volume resistivity of the first metal layer 20. According to the embodiment, it is considered that if the Lotgering factor of Al(111) is 0.8 or more, the volume resistivity of the first metal layer 20 can be set to 4 μΩ·cm or less, and a current collector with lower resistance can be realized.
[0143] When the first metal layer 20 is formed by vacuum deposition, the first metal layer 20 tends to be more (111) oriented as the pressure decreases. These examples and reference examples show that the current collector of this embodiment has excellent electrolyte resistance by satisfying the relationship of formula (1).
[0144] Industrial Applicability
[0145] The electrode for the power storage device of the embodiment of the present disclosure is useful in the power supply of various electronic devices, motors, etc. The power storage device of the embodiment of the present disclosure can be applied to the power supply of vehicles represented by bicycles and passenger cars, the power supply of communication equipment represented by smartphones, the power supply of various sensors, and the power supply of unmanned eXtended Vehicle (UxV).
Claims
1. A current collector, wherein: have: a resin layer having a first surface and a second surface located on the opposite side of the first surface; and a first metal layer, which is located on the first surface, The first metal layer contains aluminum as a main component, The thickness d of the first metal layer is not less than 0.5 μm and not more than 3 μm, In the measurement of the first metal layer based on the X-ray diffraction method, when the peak intensity ratio B / A of the intensity A of the highest X-ray diffraction peak in the range of the diffraction angle 2θ being 36° to 41° to the intensity B of the highest X-ray diffraction peak in the range of the diffraction angle 2θ being 43° to 48° is set to r, d and r satisfy the following formula (1):
2. The current collector according to claim 1, wherein The d is not less than 0.7 μm and not more than 2 μm, The d and the r satisfy the following formula (2):
3. The current collector according to claim 1 or 2, wherein The highest X-ray diffraction peak in the range of the diffraction angle 2θ of 36° to 41° is a peak of the (111) plane of aluminum, The orientation index of the (111) plane of aluminum in the first metal layer in a direction perpendicular to the first plane of the resin layer based on the Lotgering method is 0.8 or more.
4. The current collector according to any one of claims 1 to 3, wherein The intensity B of the highest X-ray diffraction peak in the range of the diffraction angle 2θ of 43° to 48° is approximately the same as the intensity of the base line in the measurement by the X-ray diffraction method.
5. The current collector according to any one of claims 1 to 4, wherein The r satisfies the following formula (3): r<1 (3)。 6. The current collector according to any one of claims 1 to 5, wherein further comprising a second metal layer located on the second surface, The second metal layer contains aluminum as a main component, The thickness d' of the second metal layer is not less than 0.5 μm and not more than 3 μm, In the measurement of the second metal layer based on the X-ray diffraction method, when the peak intensity ratio B' / A' of the intensity A' of the highest X-ray diffraction peak in the range of the diffraction angle 2θ being 36° to 41° and the intensity B' of the highest X-ray diffraction peak in the range of the diffraction angle 2θ being 43° to 48° is set as r', d' and r' satisfy the following formula (4):
7. The current collector according to any one of claims 1 to 6, wherein The resin layer includes at least one selected from polyethylene terephthalate, polypropylene, polyamide, polyimide, polyethylene, polystyrene, phenolic resin and epoxy resin.
8. An electrode for an electric storage device, wherein: have: The current collector according to any one of claims 1 to 5; and An active material layer is located on the first metal layer of the current collector.
9. An electrode for an electric storage device, wherein: have: The current collector according to claim 6; a first active material layer located on the first metal layer of the current collector; and A second active material layer is located on the second metal layer of the current collector.
10. A lithium ion secondary battery, wherein: have: A positive electrode comprising the electrode for a power storage device according to claim 8 or 9; A negative electrode comprising a negative electrode active material layer and a negative electrode current collector; a separator disposed between the negative electrode and the positive electrode; and A non-aqueous electrolyte containing lithium ions.
Citation Information
Patent Citations
Battery connections and metallized film components in energy storage devices having internal fuses
US20200373584A1