Multifunctional joint lubricating material with anti-inflammatory activity as well as preparation method and application thereof
By modifying the surface of Ti3C2 with GOx and loading manganese dioxide quantum dots, a two-dimensional/zero-dimensional coupled structure was constructed, which solved the problem of poor dispersibility of Ti3C2 in water, realized the controlled release of drugs and elimination of reactive oxygen species, provided long-lasting lubrication and anti-inflammatory effects, and solved the problem of lubrication/anti-inflammatory synergistic treatment of osteoarthritis.
Patent Information
- Application Number
- CN202411049230.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-01
AI Technical Summary
Existing Ti3C2 exhibits poor dispersibility in water, cannot achieve long-term stability, cannot effectively load drugs, and cannot eliminate reactive oxygen species at arthritic sites, resulting in poor lubrication and limiting its application in the fields of biology and joint lubrication.
By pretreating glucose oxidase (GOx) to adjust its molecular structure and modifying it onto the surface of Ti3C2, manganese dioxide quantum dots and anti-inflammatory drugs are loaded to construct a two-dimensional/zero-dimensional coupled structure, enabling controlled drug release and elimination of reactive oxygen species. Combined with photothermal conversion properties, a multifunctional joint lubricating material is formed.
It achieves good dispersibility and stability of Ti3C2 in water, and has the functions of long-lasting lubrication, high-efficiency drug loading and controllable release. It can effectively eliminate reactive oxygen species, synergistically treat osteoarthritis, reduce wear and tear, and prolong joint life.
Smart Images

Figure CN118873756A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials and biomedicine, and specifically relates to a multifunctional joint lubricating material with anti-inflammatory activity and a preparation method and application thereof. Background Art
[0002] Osteoarthritis is the most common chronic joint disease and one of the few chronic aging diseases. Osteoarthritis is a typical "wear-and-tear" joint disease caused by insufficient lubrication. Its occurrence and development are affected by many factors, and the destruction of articular cartilage on the joint surface and inflammation of the joint capsule are its main characteristics. According to the development of osteoarthritis, traditional treatment methods mainly include injection of viscoelastics such as hyaluronic acid, oral anti-inflammatory drugs and joint replacement. Due to the lack of blood vessels in the articular cartilage, oral anti-inflammatory drugs cannot be absorbed quickly and may also increase the burden on other organs. This traditional treatment method is single and cannot achieve anti-inflammatory and lubricating synergistic treatment, so the treatment efficiency is not ideal. On the other hand, due to the influence of reactive oxygen and free radicals produced by inflammation in the arthritis part, hyaluronic acid is easily degraded and loses its lubricating effect, and repeated and frequent injections of lubricants such as hyaluronic acid increase the risk of infection and economic burden on patients. Therefore, in order to improve the quality of life and treatment effect of osteoarthritis patients and avoid unnecessary pain as much as possible, it is urgent to develop new lubricating / anti-inflammatory synergistic treatment drugs.
[0003] Titanium carbide (Ti3C2) is a new type of two-dimensional nanobiomaterial with excellent properties such as good biocompatibility, large specific surface area, and good lubrication effect. It has broad application prospects in the field of biomedicine. However, in water, physiological solutions and complex physiological environments, Ti3C2 has poor dispersibility and cannot achieve long-term effective dispersion stability, so it is impossible to achieve effective drug loading and controlled release. In addition, Ti3C2 cannot eliminate the active oxygen in the inflammatory part, and its lubrication effect in water is poor, which seriously limits its application in the fields of biology and joint lubrication. At present, there is no relevant technology to achieve good dispersion and stable lubrication of Ti3C2 in joint lubrication media, and there is also a lack of preparation methods for Ti3C2-based drug loading and controlled release, anti-inflammatory, active oxygen elimination, and bone and joint synergistic lubrication. Summary of the invention
[0004] In order to solve the problems existing in the current Ti3C2 application in the biological field and joint lubrication, the present invention provides a multifunctional Ti3C2-based lubricating material and its preparation method and application. After the molecular structure of glucose oxidase (GOx) is adjusted and the catalytic activity is reduced by pretreatment technology, it is modified on the surface of Ti3C2 by gradient reaction method, which significantly improves its dispersibility and stability in various solvents such as water, has good photothermal conversion performance, and realizes the controllable loading and responsive release of various anti-inflammatory drugs.
[0005] After loading manganese dioxide quantum dots onto the Ti3C2 surface, a two-dimensional / zero-dimensional coupling and organic / inorganic hybrid structure of two-dimensional nanosheets and zero-dimensional quantum dots was constructed. This system has a good synergistic lubrication effect, which can significantly reduce the friction and wear between the friction pairs and achieve long-term lubrication. Manganese dioxide quantum dots can effectively eliminate the active oxygen in the arthritis area, synergize the photothermal induced by near-infrared light and the anti-inflammatory properties of anti-inflammatory drugs, achieve effective treatment of osteoarthritis and relieve pain in patients.
[0006] The technical solution adopted by the present invention is: Using the two-dimensional material Ti3C2, the pretreated GOx was modified and then loaded with manganese dioxide quantum dots and anti-inflammatory drugs to construct a new multifunctional joint lubricating material, which can realize photothermal conversion, drug controlled release, reactive oxygen elimination, and long-term lubrication under near-infrared response, thereby achieving synergistic treatment of osteoarthritis.
[0007] The method for preparing the multifunctional joint lubricating material with anti-inflammatory activity comprises the following steps: (1) After pretreatment of GOx, Ti3C2 was controllably modified using a gradient reaction method to prepare a Ti3C2 solution with good dispersion.
[0008] (2) Manganese dioxide quantum dots are loaded onto Ti3C2 nanosheets to prepare a zero-dimensional / two-dimensional coupled composite structure.
[0009] (3) Anti-inflammatory drugs were loaded onto Ti3C2 nanosheets to prepare a nanodrug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0010] Furthermore, in step (1), GOx is slowly heated during pretreatment, with a heating rate of 1-5 °C / min, the temperature is raised to 70-100 °C, and the reaction time is maintained for 2-8 h; The GOx is added to the Ti3C2 solution in 3 to 5 times; The mass volume ratio of the Ti3C2, GOx and deionized water is 100 mg:0.5 mg:20 mL.
[0011] Furthermore, in step (2), the quantum dots containing manganese dioxide have a size of 1 to 200 nm; The mass ratio of the Ti3C2 and MnO2-QDs is 100 mg:0.04 mg.
[0012] Furthermore, in step (3), the mass ratio of Ti3C2 to the anti-inflammatory drug is 100 mg:8 mg.
[0013] The invention provides application of the multifunctional joint lubricating material with anti-inflammatory activity in joint lubricating medicines.
[0014] The invention provides application of the multifunctional joint lubricating material with anti-inflammatory activity in drug loading.
[0015] Preferably, the multifunctional joint lubricating material with anti-inflammatory activity is loaded with anti-inflammatory drugs.
[0016] The invention provides a method for loading anti-inflammatory drugs on a multifunctional joint lubricating material with anti-inflammatory activity.
[0017] The invention also provides the friction reducing application of the multifunctional joint lubricating material with anti-inflammatory activity.
[0018] Furthermore, the anti-inflammatory drug can be a mixture of one or more drugs having anti-inflammatory effects, such as diclofenac sodium, celecoxib, meloxicam, loxoprofenal and other non-steroidal anti-inflammatory drugs.
[0019] Beneficial results of this invention: (1) After using pretreatment technology to adjust the molecular structure and catalytic activity of GOx, GOx was modified onto the surface of Ti3C2 two-dimensional nanosheets through a gradient reaction method. For the first time, the problem of poor dispersibility and instability of titanium carbide in water was solved by enzyme modification.
[0020] (2) Innovatively modifying manganese dioxide quantum dots onto Ti3C2 two-dimensional nanosheets to construct a new inorganic / organic hybrid, zero-dimensional / two-dimensional structure coupled composite lubricating material, giving full play to the synergistic effect of zero-dimensional material rolling lubrication and two-dimensional material sliding lubrication, and for the first time giving Ti3C2 lubricating material the ability to eliminate active oxygen.
[0021] (3) This lubricating material has a high drug loading capacity and excellent photothermal conversion performance. It can achieve efficient loading of a variety of anti-inflammatory drugs and controlled release under near-infrared irradiation. At the same time, it can also exhibit excellent wear-reducing performance in joint lubrication. (4) For the first time, the lubrication / anti-inflammatory synergistic treatment of Ti3C2 nanomaterials in the treatment of osteoarthritis was realized, which not only reduced joint wear and prolonged joint life, but also solved the problems of slow drug absorption and poor reactive oxygen scavenging ability, providing a new treatment method and technology for the treatment of osteoarthritis. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Catalytic activity diagram of glucose oxidase before and after pretreatment; Figure 2 Transmission electron microscopy image of the sample of glucose oxidase modified titanium carbide (Ti3C2-GOx); Figure 3This is the dispersion effect diagram of Ti3C2-GOx-MnO2-QDs; Figure 4 Zeta potential data of Ti3C2, Ti3C2-GOx and Ti3C2-GOx- MnO2-QDs; Figure 5 Photothermal test diagram of water and Ti3C2-GOx- MnO2-QDs; Figure 6 The reciprocating friction curves of H2O, Ti3C2 and Ti3C2-GOx- MnO2-QDs under the conditions of load 5 N and frequency 1 Hz; Figure 7 The infrared spectra before and after drug loading; Figure 8 Cytotoxicity diagram for lubricating materials; Fig. 9 The graph shows the protective effect on inflammation-induced chondrocyte degeneration. DETAILED DESCRIPTION
[0023] In order to better understand the essence of the present invention, the technical solution of the present invention is further described below through specific embodiments.
[0024] Example 1 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it. Set the heating rate to 5 °C / min, raise the temperature to 90 °C, and maintain the reaction time for 5 h.
[0025] (2) Add 50 mg of Ti3C2 into 10 mL of deionized water and ultrasonically shake until dissolved. Add 0.25 mg of GOx pretreated in (1) into the Ti3C2 solution in three portions.
[0026] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0027] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of sodium diclofenac, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0028] Example 2 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it at a heating rate of 5 °C / min to 100 °C, and maintain the reaction time for 5 h.
[0029] (2) Add 50 mg of Ti3C2 into 10 mL of deionized water and ultrasonically shake until dissolved. Add 0.25 mg of GOx pretreated in (1) into the Ti3C2 solution in three portions.
[0030] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0031] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of sodium diclofenac, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0032] Example 3 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it at a heating rate of 5 °C / min to 70 °C, and maintain the reaction time for 8 h.
[0033] (2) Add 50 mg of Ti3C2 into 10 mL of deionized water and ultrasonically shake until dissolved. Add 0.25 mg of GOx pretreated in (1) into the Ti3C2 solution in four portions.
[0034] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0035] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of sodium diclofenac, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0036] Example 4 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it. Set the heating rate to 5 °C / min, raise the temperature to 80 °C, and maintain the reaction time for 5 h.
[0037] (2) Add 50 mg of Ti3C2 into 10 mL of deionized water and ultrasonically shake until dissolved. Add 0.25 mg of GOx pretreated in (1) into the Ti3C2 solution in 5 portions.
[0038] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0039] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of sodium diclofenac, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0040] Example 5 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it. Set the heating rate to 5 °C / min, raise the temperature to 90 °C, and maintain the reaction time for 5 h.
[0041] (2) Add 50 mg Ti3C2 into 10 mL deionized water and ultrasonically shake until dissolved. Add 0.25 mg GOx pretreated in (1) into the Ti3C2 solution in four portions.
[0042] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0043] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of celecoxib, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of the precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0044] Example 6 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it. Set the heating rate to 1 °C / min, raise the temperature to 80 °C, and maintain the reaction time for 6 h.
[0045] (2) Add 50 mg of Ti3C2 into 10 mL of deionized water and ultrasonically shake until dissolved. Add 0.25 mg of GOx pretreated in (1) into the Ti3C2 solution in three portions.
[0046] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0047] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of sodium diclofenac, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0048] Example 7 (1) Pretreatment of GOx: Place GOx in an oven and slowly heat it. Set the heating rate to 2 °C / min, raise the temperature to 90 °C, and maintain the reaction time for 4 h.
[0049] (2) Add 50 mg of Ti3C2 into 10 mL of deionized water and ultrasonically shake until dissolved. Add 0.25 mg of GOx pretreated in (1) into the Ti3C2 solution in 5 portions.
[0050] (3) Add 0.02 mg MnO2-QDs to the Ti3C2 solution in (2) and stir together.
[0051] (4) The Ti3C2 solution prepared in (3) was mixed with 4 mg of sodium diclofenac, stirred in the dark for 24 h, centrifuged at 9000 rpm for 10 min, the supernatant was removed, and a small amount of precipitate was transferred to a beaker for freeze-drying to prepare a nano drug delivery system with controllable drug loading and responsive drug release under near-infrared light irradiation.
[0052] like Figure 1 As shown, the molecular structure of GOx after pretreatment at different temperatures is adjusted and the catalytic activity is reduced, so it can be used as a reagent to modify Ti3C2.
[0053] Ti3C2 and Ti3C2-GOx prepared in Example 1 were scanned by transmission electron microscope. Figure 2 It can be seen that the structure of titanium carbide modified by glucose oxidase was not destroyed, and the lamellar structure remained unchanged.
[0054] The dispersion effect of Ti3C2-GOx-MnO2-QDs was tested. Figure 3 The three reagent bottles in (I), (II), and (III) are the dispersion conditions after ultrasonic dissolution, standing for 30 min, and standing for 60 min. (I), (II), and (III) are 5 mg / mL Ti3C2, 5 mg / mL Ti3C2-GOx-MnO2-QDs of GOx added at one time, and 5 mg / mL Ti3C2-GOx-MnO2-QDs of GOx added in batches. In comparison, 5 mg / mL Ti3C2-GOx-MnO2-QDs of GOx added in batches has the best dispersion and lasts the longest. The infrared spectra of DS and Ti3C2-GOx-MnO2-QDs-DS are shown in Figure 7 The characteristic stretching vibration peaks of diclofenac sodium are shown at 1450 cm -1 and 1573 cm -1These peaks are mainly related to the symmetric and asymmetric carboxylate stretching vibrations, and these two characteristic peaks can be clearly seen in the Ti3C2-GOx-MnO2-QDs after loading with diclofenac sodium, proving that the carrier in the present invention can achieve the loading of anti-inflammatory drugs.
[0055] Zeta potential data of Ti3C2 and Ti3C2-GOx-MnO2-QDs are shown in Figure 4 As shown, it is demonstrated that the present invention realizes the effectiveness of surface modification of Ti3C2, so that the dispersibility of Ti3C2 in aqueous solution is improved.
[0056] Ti3C2-GOx-MnO2-QDs have good photothermal conversion performance and water solubility, and have application potential in drug loading and joint lubrication.
[0057] Photothermal test of water and Ti3C2-GOx-MnO2-QDs Figure 5 As shown in the figure, the temperature of Ti3C2-GOx-MnO2-QDs rose to 69.3 °C within 5 minutes, and the temperature continued to rise with time, which shows that Ti3C2-GOx has good photothermal conversion performance and has great potential in the future drug release and pain relief for osteoarthritis patients.
[0058] PE balls and zirconia plates were used as friction pairs, and the tribological properties of PE balls as synovial fluid additives were evaluated on a TRB-3 reciprocating friction tester. Under the conditions of load 5 N and frequency 1 Hz, the reciprocating friction curves of H2O, Ti3C2 and Ti3C2-GOx-MnO2-QDs are shown in Figure 2. Figure 6 The friction coefficient of pure water is about 0.2, and the friction coefficient of titanium carbide is about 0.09. After the addition of glucose oxidase and manganese dioxide quantum dots, the friction coefficient drops to about 0.039, and the low friction coefficient can be maintained for a long time, thus reflecting good lubrication performance.
[0059] The cytotoxicity test of lubricating materials was carried out using MTT cell counting technology. The test results are as follows: Figure 8 As shown in the figure, at both low and high concentrations, the cell survival rate was close to 100%, indicating that Ti3C2-GOx-MnO2-QDs had good biocompatibility.
[0060] H2O2 was used to establish an oxidative stress environment to induce OA and quantitative real-time polymerase chain reaction (qRT-PCR) analysis was used to track the expression levels of different mRNAs to test the protective effects of Ti3C2-GOx-MnO2-QDs on degradation and inflammation inhibition under NIR irradiation. The test data are shown in Figure 2. Fig. 9, and found that the lubricating material has an effective protective effect on cartilage under oxidative stress by upregulating Col2α and ACAN genes, thus preventing chondrocyte degradation. The above results indicate that the multifunctional joint lubricating material with anti-inflammatory activity has practical application value in joint lubrication and arthritis treatment systems.
Claims
1. A multifunctional joint lubricating material with anti-inflammatory activity, characterized in that: The joint lubricating material is obtained by pretreating glucose oxidase, modifying titanium carbide, and loading manganese dioxide quantum dots and anti-inflammatory drugs.
2. A method for preparing a multifunctional joint lubricating material with anti-inflammatory activity according to claim 1, characterized in that: Use the following steps: (1) After pre-treating GOx, Ti3C2 is controllably modified by a gradient reaction method to prepare a Ti3C2 solution with good dispersion; (2) Loading manganese dioxide quantum dots onto Ti3C2 nanosheets to prepare a zero-dimensional / two-dimensional coupled composite structure; (3) Anti-inflammatory drugs are loaded onto Ti3C2 nanosheets to prepare a multifunctional joint lubricating material with anti-inflammatory activity.
3. The preparation method according to claim 2, characterized in that During the GOx pretreatment in step (1), the GOx is slowly heated at a heating rate of 1-5 °C / min, the temperature is raised to 70-100 °C, and the reaction time is maintained for 2-8 h; The GOx is added to the Ti3C2 solution in 3 to 5 times; The mass volume ratio of the Ti3C2, GOx and deionized water is 100 mg:0.5 mg:20 mL.
4. The preparation method according to claim 2, characterized in that: In step (2), the quantum dot size of manganese dioxide is 1 to 200 nm; The mass ratio of the Ti3C2 and MnO2-QDs is 100 mg:0.04 mg.
5. The preparation method according to claim 3, characterized in that: In step (3), the mass ratio of Ti3C2 to the anti-inflammatory drug is 100 mg:8 mg.
6. Use of the multifunctional joint lubricating material with anti-inflammatory activity according to claim 1 and / or the multifunctional joint lubricating material with anti-inflammatory activity prepared by the preparation method according to any one of claims 2 to 5, characterized in that: The multifunctional joint lubricating material with anti-inflammatory activity is used for drug loading.
7. The use according to claim 6, characterized in that: The medicine is an anti-inflammatory medicine.
8. The use according to claim 7, characterized in that: The loaded drug is a single anti-inflammatory drug or a combination of anti-inflammatory drugs.
9. The use according to claim 7, characterized in that: The loaded drug is one or more of diclofenac sodium, celecoxib, meloxicam, and loxoprofenal.
10. Use of the multifunctional joint lubricating material with anti-inflammatory activity according to claim 1 and / or the multifunctional joint lubricating material with anti-inflammatory activity prepared by the preparation method according to any one of claims 2 to 5, characterized in that: The multifunctional joint lubricating material with anti-inflammatory activity is applied to joint lubrication and arthritis treatment systems.