Preparation method of caprolactam ammonolysis catalyst
By using carbon molecular sieve support and acid treatment technology in the preparation of caprolactam ammonia catalyst, the activity and product purity of the catalyst are improved, the problem of low product purity in the prior art is solved, and efficient catalytic effect and energy consumption reduction are achieved.
Patent Information
- Application Number
- CN202411019006.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-29
AI Technical Summary
In the prior art, the purity of the product 6-aminocapronitrile in the catalytic hexadiene catalyst is low in the process of catalyzing hexadiene, resulting in the need for further purification, which increases production cost and energy consumption.
Carbon molecular sieve is used as a carrier to support the active components by impregnation method and acid treatment is carried out to improve the acidic sites and activity of the molecular sieve, and the recombinant generated in the reaction are adsorbed, and the purity of the product is improved. The specific steps include heat treatment and acid treatment in an inert gas atmosphere to form the target catalyst.
The conversion rate of caprolactam is improved to more than 80%, the product selectivity is increased to more than 90%, and the purity of 6-amine capronitrile is improved, reducing separation energy consumption.
Abstract
Description
Technical Field
[0001] The invention belongs to a method for synthesizing organic compounds, and relates to a method for preparing a catalyst for ammonolysis of caprolactam. Background Art
[0002] Hexamethylenediamine is a strongly alkaline organic diamine. As an important chemical intermediate, it can be used to produce polyhexamethylenediamine adipamide (nylon 66) and hexamethylenediamine sebacamide (nylon 610), and then made into various chemical products such as nylon fibers, nylon resins and engineering plastics. According to the research on "Overall Scale of Global Hexamethylenediamine Industry in 2023, Market Share and Ranking of Major Enterprises at Home and Abroad", the global market sales of hexamethylenediamine reached 47.4 billion yuan in 2022, and it is expected to reach 68.1 billion yuan in 2029, with a compound annual growth rate (CAGR) of 5.0% (2023-2029). The traditional method for preparing hexamethylenediamine adopts the catalytic hydrogenation process of adiponitrile, and most large-scale manufacturers of hexamethylenediamine currently adopt this method. In order to avoid the use of raw material hexamethylenediamine, some manufacturers prepare hexamethylenediamine by hydrogenation reduction of 6-aminocapronitrile, which can be obtained by ammonolysis of caprolactam, which has a wide range of sources. Therefore, caprolactam ammonolysis catalyst has become a hot research topic in the field.
[0003] The patent document with publication number CN111672526A discloses a method for preparing a catalyst for synthesizing 6-aminocapronitrile, an intermediate of hexamethylenediamine, wherein the catalyst is obtained by mixing, molding, calcining, modifying and calcining a carrier, a binder, water and a peptizing agent. The patent document with publication number CN114643068A discloses a method for preparing a catalyst for preparing 6-aminocapronitrile by ammoniation of caprolactam, wherein the catalyst is mixed with an aluminum compound as a carrier, a binder and a solvent, and then mixed with a modifier solution, extruded and calcined to obtain the catalyst. The patent document with publication number CN113402418A discloses a method for preparing 6-aminocapronitrile. The method directly uses phosphoric acid or phosphate as a catalyst to catalyze the reaction of caprolactam and ammonia to prepare 6-aminocapronitrile. The patent document with publication number CN116265084A discloses a catalyst for preparing 6-aminocapronitrile by ammoniation of caprolactam, wherein the catalyst obtains a porous γ-Al2O3 catalyst by adjusting the aluminum source, the additive ratio and the crystallization time. The above preparation method focuses on improving the conversion rate of caprolactam, but ignores the purity of the product 6-aminocapronitrile. The obtained 6-aminocapronitrile needs to be further purified before it can be used to prepare hexamethylenediamine. Summary of the invention
[0004] In order to solve the technical problems existing in the prior art, the present invention provides a preparation method for a catalyst for the ammonolysis of caprolactam. After the molecular sieve is treated with acid, the acid sites of the molecular sieve are increased and the activity of the molecular sieve is improved. The molecular sieve carrier is a carbon molecular sieve, which can adsorb part of the heavy components generated during the reaction, thereby improving the purity of 6-aminocapronitrile in the product and reducing the separation energy consumption.
[0005] The technical solution adopted by the present invention is: a method for preparing a catalyst for ammonolysis of caprolactam, comprising the following steps: (1) loading the active component onto the carrier by an impregnation method to obtain catalyst A; (2) In an inert gas atmosphere, heat-treating catalyst A at 600-800 °C for 4-20 h to obtain catalyst B; (3) treating catalyst B with hydrochloric acid or nitric acid at a mass concentration of 5-35% at 30-80° C. for 0.5-6 h, repeating the acid treatment step 1-5 times, filtering, and drying in an inert gas atmosphere to obtain catalyst C; (4) In an inert gas atmosphere, heat-treating catalyst C at 500-600 °C for 3-12 h to obtain target catalyst D; The carrier is a carbon molecular sieve or a mixture of a carbon molecular sieve and at least one of pure silicon, pure aluminum, and silicon-aluminum molecular sieve; The active component is one or more of borate, phosphate and pyrophosphate.
[0006] In some specific preparation methods for the catalyst for ammonolysis of caprolactam, when the carrier is a mixture, the mass fraction of the carbon molecular sieve in the mixture is 60-100%.
[0007] Some specific methods for preparing catalysts for the ammonolysis of caprolactam are characterized in that the carrier is a carbon molecular sieve and the active component is a borate.
[0008] Some specific preparation methods for caprolactam ammonolysis catalysts are characterized in that the mass ratio of active component to carrier is 0.1~0.3:1, the concentration range of hydrochloric acid is 0.1~5.0 mol / L, the concentration range of nitric acid is 1~12 mol / L, the acid treatment time is 1~6h, and the volume of acid is 20~40 times the volume of catalyst B.
[0009] Some specific preparation methods for caprolactam ammonolysis catalysts are characterized in that the mass ratio of active component to carrier is 0.15-0.25:1, and the volume of hydrochloric acid or nitric acid is 25-35 times the volume of catalyst B.
[0010] Some specific methods for preparing catalysts for the ammonolysis of caprolactam are characterized in that the inert gas is one or more of nitrogen, argon and helium.
[0011] Some specific preparation methods for the catalyst for ammonolysis of caprolactam are characterized in that the feeding method during the acid treatment process is preferably bottom-in and top-out.
[0012] The catalyst prepared by the method for preparing the catalyst for ammonolysis of caprolactam.
[0013] Beneficial effects of the invention: The invention provides a method for preparing a catalyst for ammonolysis of caprolactam, wherein the method uses a carbon molecular sieve as a main carrier, loads an active component on the carrier by an impregnation method, and then obtains a target catalyst by an acid treatment process. The catalyst can achieve a caprolactam conversion rate of more than 80% and a product selectivity of more than 90% in the catalytic caprolactam ammonolysis reaction, and can also improve the purity of the product. DETAILED DESCRIPTION
[0014] The present invention is described in detail below with reference to specific embodiments. The raw materials and reagents used in the embodiments are commercially available chemical raw materials and reagents unless otherwise specified, the carbon molecular sieve complies with the HG∕T 4364-2020 standard, the pure silicon molecular sieve is synthesized according to Example 4 of the patent 201910340428.3, and the aluminum oxide is purchased from Sasol.
[0015] Example 1: 180 g of carbon molecular sieve was added to 400 ml of 10% sodium borate aqueous solution, immersed at room temperature for 1.5 h, filtered, washed with water, and dried at 60 °C to obtain catalyst A1; the obtained catalyst A1 was placed in a roasting furnace and heat treated at 700 °C in an argon atmosphere for 8 h to obtain catalyst B1; then catalyst B1 was added to 7.5 L of 3 mol / L hydrochloric acid solution, heated to 50 °C for acid treatment for 3 h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60 °C in an argon atmosphere to obtain catalyst C1. Catalyst C1 was heat treated at 550 °C in a roasting furnace for 5 h to obtain the target catalyst D1.
[0016] Example 2: 180 g of carbon molecular sieve was added to 400 ml of 10% sodium borate aqueous solution, immersed at room temperature for 2.0 h, filtered, washed with water, and dried at 60 °C to obtain catalyst A2; the obtained catalyst A2 was placed in a roasting furnace and heat-treated at 600 °C in an argon atmosphere for 18 h to obtain catalyst B2; then catalyst B2 was added to 9 L of 3 mol / L hydrochloric acid solution, heated to 35 °C for acid treatment for 5 h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 65 °C in an argon atmosphere to obtain catalyst C2. Catalyst C2 was heat-treated at 600 °C in a roasting furnace for 3 h to obtain the target catalyst D2.
[0017] Example 3: 180 g of carbon molecular sieve was added to 400 ml of 5% sodium borate aqueous solution, immersed at room temperature for 3 h, filtered, washed with water, and dried at 60 °C to obtain catalyst A3; the obtained catalyst A3 was placed in a roasting furnace and heat treated at 800 °C in an argon atmosphere for 5 h to obtain catalyst B3; then catalyst B3 was added to 9 L of 3 mol / L hydrochloric acid solution, heated to 65 °C for acid treatment for 1 h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60 °C in an argon atmosphere to obtain catalyst C3. Catalyst C3 was heat treated at 500 °C in a roasting furnace for 11 h to obtain the target catalyst D3.
[0018] Example 4: 180 g of carbon molecular sieve was added to 400 ml of 20% sodium borate aqueous solution, immersed at room temperature for 2 h, filtered, washed with water, and dried at 60 °C to obtain catalyst A4; the obtained catalyst A4 was placed in a roasting furnace and heat-treated at 670 °C in an argon atmosphere for 10 h to obtain catalyst B4; then catalyst B4 was added to 10.8 L of 3 mol / L hydrochloric acid solution, heated to 80 °C for acid treatment for 4 h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60 °C in an argon atmosphere to obtain catalyst C4. Catalyst C4 was heat-treated at 550 °C in a roasting furnace for 5 h to obtain target catalyst D4.
[0019] Example 5: 180 g of carbon molecular sieve was added to 400 ml of 15% sodium borate aqueous solution, immersed at room temperature for 10 h, filtered, washed with water, and dried at 60 °C to obtain catalyst A5; the obtained catalyst A5 was placed in a roasting furnace and heat treated at 700 °C in an argon atmosphere for 4 h to obtain catalyst B5; then catalyst B5 was added to 9 L of 3 mol / L hydrochloric acid solution, heated to 30 °C for acid treatment for 1 h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60 °C in an argon atmosphere to obtain catalyst C5. Catalyst C5 was heat treated at 600 °C in a roasting furnace for 7 h to obtain the target catalyst D5.
[0020] Example 6: 180 g of carbon molecular sieve was added to 400 ml of 10% sodium pyrophosphate aqueous solution, immersed at room temperature for 1.5 h, filtered, washed with water, and dried at 60 °C to obtain catalyst A6; the obtained catalyst A6 was placed in a roasting furnace and heat treated at 700 °C in an argon atmosphere for 8 h to obtain catalyst B6; then catalyst B6 was added to 9 L of 3 mol / L hydrochloric acid solution, heated to 50 °C for acid treatment for 3 h, filtered, washed with water, and dried at 60 °C in an argon atmosphere to obtain catalyst C6. Catalyst C6 was heat treated at 550 °C in a roasting furnace for 5 h to obtain the target catalyst D6.
[0021] Example 7: 130 g of carbon molecular sieve and 50 g of pure silicon molecular sieve were mechanically extruded into a cylinder with a diameter of 3 mm and a length of 15-20 mm, added to 400 ml of a 10% sodium borate aqueous solution by mass, immersed at room temperature for 1.5 h, filtered, washed with water, and dried at 60°C to obtain catalyst A7; the obtained catalyst A7 was placed in a roasting furnace and heat-treated at 700°C for 8 h in an argon atmosphere to obtain catalyst B7; then catalyst B7 was added to 9 L of a 3 mol / L hydrochloric acid solution, heated to 50°C for acid treatment for 3 h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60°C in an argon atmosphere to obtain catalyst C7. Catalyst C7 was heat-treated at 550°C in a roasting furnace for 5 h to obtain the target catalyst D7.
[0022] Example 8: 150 g of carbon molecular sieve and 30 g of pure silicon molecular sieve were mechanically extruded into a cylinder with a diameter of 3 mm and a length of 15-20 mm, added to 400 ml of a 10% sodium borate aqueous solution, immersed at room temperature for 1.5 h, filtered, washed with water, and dried at 60°C to obtain catalyst A8; the obtained catalyst A8 was placed in a roasting furnace and heat-treated at 700°C for 8 h in an argon atmosphere to obtain catalyst B8; then catalyst B8 was added to 9 L of a 3 mol / L hydrochloric acid solution, heated to 50°C for acid treatment for 3 h, filtered, washed with water, and dried at 60°C in an argon atmosphere to obtain catalyst C8. Catalyst C8 was heat-treated at 550°C in a roasting furnace for 5 h to obtain target catalyst D8.
[0023] Example 9: 150 g of carbon molecular sieve and 30 g of aluminum oxide were mechanically extruded into a cylinder with a diameter of 3 mm and a length of 15-20 mm, added to 400 ml of a 10% sodium borate aqueous solution, immersed at room temperature for 1.5 h, filtered, washed with water, and dried at 60°C to obtain catalyst A9; the obtained catalyst A9 was placed in a roasting furnace and heat-treated at 600°C for 8 h in an argon atmosphere to obtain catalyst B9; then catalyst B9 was added to 9 L of a 3 mol / L hydrochloric acid solution, heated to 50°C for acid treatment for 3 h, filtered, washed with water, and dried at 60°C in an argon atmosphere to obtain catalyst C9. Catalyst C9 was heat-treated at 550°C in a roasting furnace for 5 h to obtain the target catalyst D9.
[0024] Comparative Example 1: 180g of aluminum oxide was mechanically extruded into a cylinder with a diameter of 3mm and a length of 15-20mm, added to 400ml of a 10% sodium borate aqueous solution, immersed at room temperature for 1.5h, filtered, washed with water, and dried at 60℃ to obtain catalyst A'1; the obtained catalyst A'1 was placed in a roasting furnace and heat-treated at 700℃ in an argon atmosphere for 8h to obtain catalyst B'1; then catalyst B'1 was added to 9L of a 3mol / L hydrochloric acid solution, heated to 50℃ for acid treatment for 3h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60℃ in an argon atmosphere to obtain catalyst C'1. Catalyst C'1 was heat-treated at 550℃ in a roasting furnace for 5h to obtain the target catalyst D'1.
[0025] Comparative Example 2: 180g of silicon dioxide was mechanically extruded into a cylinder with a diameter of 3mm and a length of 15-20mm, added to 400ml of a 10% sodium borate aqueous solution, immersed at room temperature for 1.5h, filtered, washed with water, and dried at 60℃ to obtain catalyst A'2; the obtained catalyst A'2 was placed in a roasting furnace and heat-treated at 700℃ in an argon atmosphere for 8h to obtain catalyst B'2; then catalyst B'2 was added to 9L of a 3mol / L hydrochloric acid solution, heated to 50℃ for acid treatment for 3h, and after cumulative treatment for 3 times, filtered, washed with water, and dried at 60℃ in an argon atmosphere to obtain catalyst C'2. Catalyst C'2 was heat-treated at 550℃ in a roasting furnace for 5h to obtain the target catalyst D'2.
[0026] Test example: Evaluation of the catalytic performance of the catalyst for the ammonolysis of caprolactam The catalysts prepared in the examples and comparative examples were used to evaluate the fixed-bed caprolactam ammonolysis reaction. 50 g of the catalyst was loaded into the fixed bed, the temperature was raised to 400 °C, and caprolactam was heated at a mass space velocity of 0.5 h -1 Feed, ammonia / caprolactam molar ratio of 30, collect liquid 6-aminocapronitrile product, sample and control, after mass balance calculation, obtain the conversion rate of raw material caprolactam and the selectivity data of product 6-aminocapronitrile, and use liquid chromatography to detect the purity of product 6-aminocapronitrile. Specific data are shown in Table 1.
[0027] Table 1 Evaluation data of the catalysts of the examples and comparative examples for the catalytic aminolysis of caprolactam catalyst Conversion rate of caprolactam Selectivity of 6-aminocapronitrile Purity of 6-aminocapronitrile D1 82.70% 99.60% 99.80% D2 82.40% 99.50% 99.70% D3 82.20% 99.45% 99.50% D4 84.30% 99.40% 99.60% D5 83.10% 99.50% 99.55% D6 81.2% 99.05% 99.20% D7 81.30% 99.30% 99.25% D8 81.80% 99.40% 99.40% D9 81.50% 99.30% 99.30% D’1 80.80% 99.00% 99.00% D’2 80.90% 99.05% 99.05% The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for ammonolysis of caprolactam, It is characterized in that The method comprises the following steps: (1) loading the active component onto the carrier by an impregnation method to obtain catalyst A; (2) In an inert gas atmosphere, heat-treating catalyst A at 600-800 °C for 4-20 h to obtain catalyst B; (3) treating catalyst B with hydrochloric acid or nitric acid at a mass concentration of 5-35% at 30-80° C. for 0.5-6 h, repeating the acid treatment step 1-5 times, filtering, and drying in an inert gas atmosphere to obtain catalyst C; (4) In an inert gas atmosphere, heat-treating catalyst C at 500-600 °C for 3-12 h to obtain target catalyst D; The carrier is a carbon molecular sieve or a mixture of a carbon molecular sieve and at least one of pure silicon, pure aluminum, and silicon-aluminum molecular sieve; The active component is one or more of borate, phosphate and pyrophosphate.
2. The method for preparing a catalyst for ammonolysis of caprolactam according to claim 1, It is characterized in that When the carrier is a mixture, the mass fraction of the carbon molecular sieve in the mixture is 60-100%.
3. The method for preparing a catalyst for ammonolysis of caprolactam according to claim 1, It is characterized in that The carrier is a carbon molecular sieve, and the active component is a borate.
4. The method for preparing a catalyst for ammonolysis of caprolactam according to any one of claims 1 to 3, It is characterized in that The mass ratio of the active component to the carrier is 0.1-0.3:1, and the volume of the hydrochloric acid or nitric acid is 20-40 times the volume of the catalyst B.
5. The method for preparing a catalyst for ammonolysis of caprolactam according to claim 4, It is characterized in that The mass ratio of the active component to the carrier is 0.15-0.25:1, and the volume of the hydrochloric acid or nitric acid is 25-35 times the volume of the catalyst B.
6. The method for preparing a catalyst for ammonolysis of caprolactam according to claim 5, It is characterized in that The concentration of hydrochloric acid is 0.1~5.0mol / L, the concentration of nitric acid is 1~12mol / L, and the time of each acid treatment is 1~6h.
7. A method for preparing a catalyst for ammonolysis of caprolactam according to any one of claims 1 to 3, Features: The inert gas is one or more of nitrogen, argon and helium.
8. The method for preparing a catalyst for ammonolysis of caprolactam according to any one of claims 1 to 3, Features: The best feeding method for the acid treatment process is bottom-in and top-out.
9. A catalyst prepared according to the method for preparing a catalyst for ammonolysis of caprolactam according to any one of claims 1 to 3.
Citation Information
Patent Citations
Preparation method for rapidly synthesizing pure silicon MCM-41 molecular sieve
CN109987613A
Preparation method of catalyst for synthesizing hexamethylenediamine intermediate 6-aminocapronitrile and synthesis method of 6-aminocapronitrile
CN111672526A
Method for preparing 6-aminocapronitrile
CN113402418A
Preparation method and application of 6-aminocapronitrile catalyst prepared by caprolactam ammonification
CN114643068A
Catalyst for preparing 6-aminocapronitrile through caprolactam ammoniation, preparation method of catalyst and application of catalyst in preparation of 6-aminocapronitrile through ammoniation
CN116265084A