Catalyst, catalytic module and preparation method and application thereof

By using mesoporous molecular sieve support and MnCeZrTi composite semiconductor materials and Ag and Pd in ​​the honeycomb catalytic module, low-cost and efficient gas purification is achieved, solving the problem of high cost of traditional precious metal catalysts and improving the purification effect.

CN118874522APending Publication Date: 2024-11-01NINGBO FOTILE KITCHEN WARE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410908921.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The supported precious metal catalysts used in traditional honeycomb catalytic modules are costly and consumed at a large amount, making it difficult to meet the needs of high discharge and high activity.

Method used

Mesoporous molecular sieve is used as a support and is loaded with MnCeZrTi composite semiconductor material and Ag and Pd to achieve efficient synergistic catalytic activity under the action of high-voltage electric field and improve the purification effect.

Benefits of technology

It realizes low-cost and efficient gas purification, reduces the amount of precious metals, improves catalytic activity and purification effect, and is suitable for gas purification systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004932974740000131
    Figure BDA0004932974740000131
  • Figure BDA0004932974740000141
    Figure BDA0004932974740000141
Patent Text Reader

Abstract

The invention relates to a catalyst, a catalytic module and a preparation method and application thereof. The catalyst comprises a composite carrier as well as Ag and Pd which are loaded on the composite carrier, and the composite carrier comprises a mesoporous molecular sieve and a MnCeZrTi composite semiconductor material loaded on the mesoporous molecular sieve. The catalyst not only has an excellent purification effect, but also is relatively low in cost, and can be widely applied to a gas purification system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of gas purification, and in particular to a catalyst, a catalytic module, and a preparation method and application thereof. Background Art

[0002] Plasma synergistic catalytic purification technology has the advantages of high purification efficiency and long service life. It can sterilize and remove odors in the refrigerator, and is an effective way to solve the odor problem in the refrigerator. Among them, the honeycomb plasma catalytic method is to achieve a high-intensity corona discharge synergistic catalytic effect by placing a honeycomb catalytic module with a catalyst coating between two high-voltage mesh electrodes. It has low wind resistance and long life, and is considered to be a high-potential purification technology. Traditional catalyst coatings used for honeycomb catalytic modules generally use supported precious metal catalysts, such as gold (Au), platinum (Pt), etc. However, in order to meet the catalytic requirements of high discharge and high activity, the amount of precious metals used is relatively high, and the mass fraction in the supported precious metal catalyst is as high as about 3%-10%, which greatly increases the cost. Summary of the invention

[0003] Based on this, it is necessary to provide a catalyst, a catalytic module and a preparation method and application thereof to address the above problems; the catalyst not only has excellent purification effect but also has low cost and can be widely used in gas purification systems.

[0004] A catalyst comprises a composite carrier and Ag and Pd loaded on the composite carrier. The composite carrier comprises a mesoporous molecular sieve and a MnCeZrTi composite semiconductor material loaded on the mesoporous molecular sieve.

[0005] In one embodiment, the total mass of Mn, Ce, Zr, and Ti elements in the MnCeZrTi composite semiconductor material is 0.5%-10% of the mass of the mesoporous molecular sieve;

[0006] And / or, in the MnCeZrTi composite semiconductor material, the molar ratio of Mn, Ce, Zr and Ti is (0.01-1):(0.01-1):(0.1-2):1.

[0007] In one embodiment, the mass of Ag is 0.1%-5% of the mass of the composite carrier;

[0008] And / or, the mass of the Pd is 0.01%-0.5% of the mass of the composite carrier.

[0009] In one embodiment, the pore size of the mesoporous molecular sieve is 2nm-50nm;

[0010] And / or, the mesoporous molecular sieve includes SBA-15.

[0011] A method for preparing the catalyst as described above comprises the following steps:

[0012] The dispersion of citric acid is mixed with a manganese source, a cerium source, a zirconium source, a titanium source and a mesoporous molecular sieve to obtain a mixture, and the mixture is dried for the first time and calcined for the first time under a protective atmosphere to obtain a composite carrier;

[0013] The dispersion containing the silver source and the palladium source is mixed with the composite carrier, and the catalyst is prepared through a second drying, a second calcination and a reduction treatment.

[0014] In one embodiment, the molar ratio of citric acid in the citric acid dispersion to the Ti element in the titanium source is (0.05-0.5):1;

[0015] And / or, in the mixture, the molar ratio of the Mn element in the manganese source, the Ce element in the cerium source, the Zr element in the zirconium source and the Ti element in the titanium source is (0.01-1):(0.01-1):(0.1-2):1;

[0016] And / or, in the mixture, the total mass of the Mn element in the manganese source, the Ce element in the cerium source, the Zr element in the zirconium source and the Ti element in the titanium source is 0.5%-10% of the mass of the mesoporous molecular sieve;

[0017] And / or, the first drying temperature is 60°C-180°C, and the time is 0.5h-5h;

[0018] And / or, the protective atmosphere includes at least one of nitrogen and argon;

[0019] And / or, the temperature of the first calcination is 300° C.-600° C., and the time is 0.5 h-5 h.

[0020] In one embodiment, in the dispersion containing the silver source and the palladium source, the mass of the Ag element in the silver source is 0.1%-5% of the mass of the composite support;

[0021] and / or, the mass of the Pd element in the palladium source is 0.01%-0.5% of the mass of the composite support;

[0022] And / or, the temperature of the second drying is 60°C-180°C, and the time is 0.5h-5h;

[0023] And / or, the second calcination temperature is 300°C-600°C, and the time is 0.5h-5h;

[0024] And / or, the reduction treatment temperature is 200° C.-600° C., the time is 0.1 h-5 h, and the reducing atmosphere includes hydrogen.

[0025] A catalytic module comprises a porous substrate and a catalyst coating distributed on the surface of the porous substrate, wherein the catalyst coating comprises the catalyst as described above.

[0026] A method for preparing the catalytic module as described above comprises the following steps:

[0027] Mixing the citric acid dispersion with a manganese source, a cerium source, a zirconium source, a titanium source and a mesoporous molecular sieve to obtain a mixture;

[0028] Placing the mixture on the surface of a porous substrate, drying it for the first time and calcining it for the first time under a protective atmosphere to obtain a prefabricated catalytic module;

[0029] A dispersion containing a silver source and a palladium source is placed on the surface of the prefabricated catalytic module, and the catalytic module is obtained through a second drying, a second calcination and a reduction treatment.

[0030] In one embodiment, the mixture further includes a binder, the binder includes aluminum sol, and the mass of the binder is 2%-15% of the mass of the mesoporous molecular sieve;

[0031] And / or, the porous substrate comprises a porous ceramic substrate;

[0032] And / or, the mixture is placed on the surface of the porous substrate by vacuum coating;

[0033] And / or, the method of placing the dispersion containing the silver source and the palladium source on the surface of the prefabricated catalytic module is selected from the impregnation method.

[0034] A gas purification system comprises the catalytic module as described above.

[0035] In the catalyst described in the present invention, a mesoporous molecular sieve is used as a basic carrier, and a MnCeZrTi composite semiconductor material and Ag and Pd are highly dispersedly loaded. The Mn, Ce, Zr and Ti elements in the MnCeZrTi composite semiconductor material have abundant oxygen vacancies due to interaction and charge balance, and can achieve efficient synergistic catalytic activity between dual active components and composite carriers with relatively cheap precious metals Ag and Pd. On the one hand, under the action of a high-voltage electric field, oxygen vacancy sites and highly dispersed Ag and Pd metal sites can effectively serve as electron transfer sites, which can ensure that the pores of the catalytic module are filled with a large number of micro-discharges, thereby generating high-intensity plasma; on the other hand, under the synergistic effect of the highly dispersed loaded Ag sites, Pd sites, Mn sites, Ce sites and abundant oxygen vacancy sites, ozone generated by catalysis can be efficiently adsorbed, and further under the synergistic effect of high-intensity plasma discharge, oxygen and ozone can be activated to generate a large number of free radicals and active oxygen species, thereby efficiently oxidizing and decomposing pollutants such as VOCs, thereby achieving an efficient purification effect. DETAILED DESCRIPTION

[0036] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0038] The invention provides a catalyst, comprising a composite carrier and Ag and Pd loaded on the composite carrier. The composite carrier comprises a mesoporous molecular sieve and a MnCeZrTi composite semiconductor material loaded on the mesoporous molecular sieve.

[0039] In the catalyst described in the present invention, a mesoporous molecular sieve is used as a basic carrier, and a MnCeZrTi composite semiconductor material and Ag and Pd are highly dispersedly loaded. The Mn, Ce, Zr and Ti elements in the MnCeZrTi composite semiconductor material have abundant oxygen vacancies due to interaction and charge balance, and can achieve efficient synergistic catalytic activity between dual active components and composite carriers with relatively cheap precious metals Ag and Pd. On the one hand, under the action of a high-voltage electric field, oxygen vacancy sites and highly dispersed Ag and Pd metal sites can effectively serve as electron transfer sites, which can ensure that the pores of the catalytic module are filled with a large number of micro-discharges, thereby generating high-intensity plasma; on the other hand, under the synergistic effect of the highly dispersed loaded Ag sites, Pd sites, Mn sites, Ce sites and abundant oxygen vacancy sites, ozone generated by catalysis can be efficiently adsorbed, and further under the synergistic effect of high-intensity plasma discharge, oxygen and ozone can be activated to generate a large number of free radicals and active oxygen species, thereby efficiently oxidizing and decomposing pollutants such as VOCs, thereby achieving an efficient purification effect.

[0040] In one embodiment, the total mass of Mn, Ce, Zr, and Ti elements in the MnCeZrTi composite semiconductor material is 0.5%-10%, preferably 2%-7%, of the mass of the mesoporous molecular sieve. By regulating the mass of the MnCeZrTi composite semiconductor material, it is beneficial to further promote its synergistic effect with Ag sites and Pd sites, thereby improving the catalytic activity and enhancing the purification effect.

[0041] In one embodiment, in the MnCeZrTi composite semiconductor material, the molar ratio of Mn, Ce, Zr and Ti is (0.01-1):(0.01-1):(0.1-2):1, preferably (0.1-0.8):(0.1-0.8):(0.5-1.5):1. By regulating the molar ratio of Mn, Ce, Zr and Ti in the MnCeZrTi composite semiconductor material, it is beneficial to further promote the synergistic effect between Mn, Ce, Zr and Ti, thereby improving the catalytic activity and enhancing the purification effect.

[0042] In one embodiment, the mass of Ag is 0.1%-5%, preferably 0.5%-2.5% of the mass of the composite carrier; the mass of Pd is 0.01%-0.5%, preferably 0.05%-0.3% of the mass of the composite carrier. By regulating the mass of Ag and Pd, it is beneficial to improve the catalytic activity and enhance the purification effect.

[0043] In one embodiment, the pore size of the mesoporous molecular sieve is 2nm-50nm. Specifically, the mesoporous molecular sieve is preferably a silicon-based molecular sieve, which includes but is not limited to SBA-15, and is more preferably SBA-15. SBA-15 has a two-dimensional hexagonal through-pore structure, and is bonded by a neutral surfactant P123 (S0) and a neutral inorganic silicon species (I0) through hydrogen bonding. There is no strong electrostatic effect, and with the further hydrolysis and condensation of silanol, short-range hexagonal colloid particles are accumulated and a skeleton is formed. It has well-developed pores, a large specific surface area, and a strong adsorption effect. As a catalytic carrier, on the one hand, the mesoporous structure of SBA-15 can highly disperse MnCeZrTi composite semiconductor materials and Ag, Pd, which is conducive to the formation of highly dispersed active sites; on the other hand, the high specific surface area of ​​SBA-15 can effectively adsorb pollutants such as VOCs to achieve an efficient purification effect.

[0044] The present invention provides a method for preparing the catalyst as described above, comprising the following steps:

[0045] The dispersion of citric acid is mixed with a manganese source, a cerium source, a zirconium source, a titanium source and a mesoporous molecular sieve to obtain a mixture, and the mixture is dried for the first time and calcined for the first time under a protective atmosphere to obtain a composite carrier;

[0046] The dispersion containing the silver source and the palladium source is mixed with the composite carrier, and the catalyst is prepared through a second drying, a second calcination and a reduction treatment.

[0047] The carbon produced by the decomposition of citric acid at high temperature captures part of the active lattice oxygen in the composite carrier and volatilizes in the form of carbon dioxide, thereby forming abundant oxygen vacancies in the composite carrier, which is not only beneficial to the subsequent dispersion of Ag and Pd on the composite carrier, but also helps to achieve efficient synergistic catalytic activity between the two active components and between the functional carriers.

[0048] In one embodiment, the molar ratio of citric acid in the citric acid dispersion to the Ti element in the titanium source is (0.05-0.5):1, preferably (0.1-0.3):1.

[0049] The solvent of the dispersion includes but is not limited to water, preferably water.

[0050] In one embodiment, in the mixture, the molar ratio of the Mn element in the manganese source, the Ce element in the cerium source, the Zr element in the zirconium source and the Ti element in the titanium source is (0.01-1):(0.01-1):(0.1-2):1, preferably (0.1-0.8):(0.1-0.8):(0.5-1.5):1.

[0051] Specifically, the manganese source is selected from soluble manganese salts, preferably Mn(NO3)2·6H2O; the cerium source is selected from soluble cerium salts, preferably Ce(NO3)3·6H2O; the zirconium source is selected from soluble zirconium salts, preferably ZrO(NO3)2; the titanium source is selected from soluble titanium salts, preferably TiCl4.

[0052] In one embodiment, in the mixture, the total mass of the Mn element in the manganese source, the Ce element in the cerium source, the Zr element in the zirconium source and the Ti element in the titanium source is 0.5%-10% of the mass of the mesoporous molecular sieve, preferably 2%-7%.

[0053] Specifically, the mesoporous molecular sieve is preferably a silicon-based molecular sieve, which includes but is not limited to SBA-15, and is more preferably SBA-15.

[0054] In one embodiment, the first drying is carried out at a temperature of 60°C-180°C, preferably 80°C-150°C, and for a time of 0.5h-5h, preferably 1h-3h.

[0055] In one embodiment, the temperature of the first calcination is 300°C-600°C, preferably 400°C-550°C; the time is 0.5h-5h, preferably 1h-4h; the protective atmosphere includes but is not limited to at least one of nitrogen and argon, preferably nitrogen and argon.

[0056] In one embodiment, the mass of the Ag element in the silver source is 0.1%-5% of the mass of the composite carrier; the mass of the Pd element in the palladium source is 0.01%-0.5% of the mass of the composite carrier; the solvent of the dispersion includes but is not limited to water, preferably water.

[0057] It is understandable that the method of preparing the silver source and the palladium source into dispersions separately and then mixing them with the composite carrier in sequence is also feasible, and the present invention does not limit this. It is preferred to directly mix the silver source and the palladium source to prepare the dispersion.

[0058] In one embodiment, the second drying is carried out at a temperature of 60°C-180°C, preferably 80°C-150°C, and for a time of 0.5h-5h, preferably 1h-3h.

[0059] In one embodiment, the second calcination temperature is 300°C-600°C, preferably 350°C-500°C; the time is 0.5h-5h, preferably 1h-5h.

[0060] In one embodiment, the reduction treatment temperature is 200°C-600°C, preferably 300°C-550°C; the time is 0.1h-5h, preferably 0.5h-3h; the reducing atmosphere includes but is not limited to hydrogen, preferably hydrogen.

[0061] The present invention provides a catalytic module, comprising a porous substrate and a catalyst coating distributed on the surface of the porous substrate, wherein the catalyst coating comprises the catalyst as described above.

[0062] Specifically, the porous substrate includes but is not limited to a porous ceramic substrate, preferably a porous ceramic substrate, which has a large surface area of ​​pores, which is conducive to increasing the loading amount of the catalyst.

[0063] The present invention provides a method for preparing the catalytic module as described above, comprising the following steps:

[0064] Mixing the citric acid dispersion with a manganese source, a cerium source, a zirconium source, a titanium source and a mesoporous molecular sieve to obtain a mixture;

[0065] Placing the mixture on the surface of a porous substrate, drying it for the first time and calcining it for the first time under a protective atmosphere to obtain a prefabricated catalytic module;

[0066] A dispersion containing a silver source and a palladium source is placed on the surface of the prefabricated catalytic module, and the catalytic module is obtained through a second drying, a second calcination and a reduction treatment.

[0067] It is understandable that the catalytic module can be obtained by directly dispersing the catalyst into a solvent and then placing it on the surface of a porous substrate and drying it. The present invention does not limit this. It is preferred to use the above method to prepare the catalyst in situ on the surface of a porous substrate.

[0068] In one embodiment, the mixture further includes a binder, which includes but is not limited to aluminum sol, preferably aluminum sol, and the mass of the binder is 2%-15% of the mass of the mesoporous molecular sieve, preferably 5%-12%.

[0069] In one embodiment, the mixture is placed on the surface of the porous substrate in a manner including but not limited to vacuum coating, preferably vacuum coating.

[0070] In one embodiment, the method of placing the dispersion containing the silver source and the palladium source on the surface of the prefabricated catalytic module includes but is not limited to the impregnation method, preferably the impregnation method.

[0071] The present invention also provides a gas purification system, comprising the catalytic module as described above. It is understandable that the catalytic component in the gas purification system comprises two electrodes and a catalytic module disposed between the two electrodes.

[0072] In the present invention, when a certain high voltage is applied between the two electrodes of the gas purification system, a full discharge will occur between the two electrodes under the action of water molecules in the air and the catalyst in the catalytic module, which is mainly manifested in that the micropores in the substrate pores and the inside of the catalyst are filled with a large number of micro-discharges. On the one hand, the metal sites on the surface of the catalyst can further increase the amount of micro-discharges and generate a large amount of plasma, including active components such as active oxygen, free radicals, high-energy electrons and ozone; on the other hand, the presence of the catalyst can also decompose ozone into active oxygen and free radicals. When the pollutant VOC gas passes through the catalytic component, it will first be decomposed by a large number of active components in the gas phase. At the same time, the VOC molecules will also be fully adsorbed and enriched by the catalyst, and adsorbed active oxygen and free radicals will be generated through catalytic oxidation under ozone and discharge environment, thereby being decomposed and removed by adsorbed free radical active oxygen. Therefore, the gas purification system can achieve efficient purification of VOC and ozone control effects.

[0073] The gas purification system provided by the present invention can be used in equipment with air ducts, such as air purifiers, refrigerators, cabinets, etc., and the present invention is not limited to this. The operation of the fan in the air duct can bring the air containing pollutants into the gas purification system for decomposition and purification, and then the clean air is discharged through the air outlet of the fan to achieve the purpose of purifying the air.

[0074] Hereinafter, the catalyst, catalytic module, preparation method and application thereof will be further described by the following specific examples. However, it will be understood by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0075] It should be noted that in the following embodiments, comparative examples and application examples, the material of the porous plate electrode is stainless steel, the thickness is controlled at about 3 mm, the pore diameter is about 2 mm, and the pore spacing is about 2.5 mm; in the porous honeycomb ceramic substrate, the ceramic pores are about 0.8 mm × 0.8 mm square, the pore density is about 300 ppi, and the substrate thickness is about 20 mm.

[0076] Example 1

[0077] Disperse citric acid in water to form a dispersion, then add Mn(NO3)2·6H2O, Ce(NO3)3·6H2O, ZrO(NO3)2 and TiCl4 and stir evenly, wherein the molar ratio of Mn, Ce, Zr and Ti elements is 0.2:0.5:1:1, and the molar ratio of citric acid to Ti element is 0.15:1; then add SBA-15 and stir thoroughly, and finally add aluminum sol to form a uniformly dispersed mixture, wherein the total mass of Mn, Ce, Zr and Ti elements is 5% of the mass of SBA-15, and the mass of aluminum sol is 5% of the mass of SBA-15.

[0078] The mixture was coated on the surface of a porous honeycomb ceramic substrate by vacuum coating, dried for a first time at 120°C for 2 hours, and then calcined for a first time at 500°C in a nitrogen environment for 3 hours to obtain a prefabricated catalytic module.

[0079] Silver nitrate and palladium nitrate are dispersed in water to form a uniform dispersion, and then the dispersion is impregnated and dispersed on the prefabricated catalytic module by an impregnation method, first dried for a second time at 120°C for 2 hours, then calcined for a second time at 400°C for 3 hours, and finally reduced at 400°C in a hydrogen environment for 2 hours to obtain a porous honeycomb catalytic coating module. According to the test, the mass of Ag in the porous honeycomb catalytic coating module is 1% of the mass of the prefabricated catalytic module, and the mass of Pd is 0.1% of the mass of the prefabricated catalytic module.

[0080] Example 2

[0081] The difference between Example 2 and Example 1 is that the total mass of Mn, Ce, Zr, and Ti elements is 0.5% of the mass of SBA-15.

[0082] Example 3

[0083] The difference between Example 3 and Example 1 is that the molar ratio of Mn, Ce, Zr and Ti elements is 0.01:0.01:0.1:1.

[0084] Example 4

[0085] The difference between Example 4 and Example 1 is that the mass of Ag in the prepared porous honeycomb catalytic coating module is 0.1% of the mass of the prefabricated catalytic module.

[0086] Example 5

[0087] The difference between Example 5 and Example 1 is that the mass of Ag in the prepared porous honeycomb catalytic coating module is 0.01% of the mass of the prefabricated catalytic module.

[0088] Example 6

[0089] Disperse citric acid in water to form a dispersion, then add Mn(NO3)2·6H2O, Ce(NO3)3·6H2O, ZrO(NO3)2 and TiCl4 and stir evenly, wherein the molar ratio of Mn, Ce, Zr and Ti elements is 1:1:2:1, and the molar ratio of citric acid to Ti element is 0.45:1; then add SBA-15 and stir thoroughly, and finally add aluminum sol to form a uniformly dispersed mixture, wherein the total mass of Mn, Ce, Zr and Ti elements is 10% of the mass of SBA-15, and the mass of aluminum sol is 10% of the mass of SBA-15.

[0090] The mixture was coated on the surface of a porous honeycomb ceramic substrate by vacuum coating, dried for a first time at 150°C for 1.5 hours, and then calcined for a first time at 400°C in a nitrogen environment for 4 hours to obtain a prefabricated catalytic module.

[0091] Silver nitrate and palladium nitrate are dispersed in water to form a uniform dispersion, and then the dispersion is impregnated and dispersed on the prefabricated catalytic module by an impregnation method, first dried for a second time at 160°C for 1 hour, then calcined for a second time at 400°C for 4 hours, and finally reduced at 500°C in a hydrogen environment for 2 hours to obtain a porous honeycomb catalytic coating module. According to the test, the mass of Ag in the porous honeycomb catalytic coating module is 5% of the mass of the prefabricated catalytic module, and the mass of Pd is 0.5% of the mass of the prefabricated catalytic module.

[0092] Example 7

[0093] The difference between Example 7 and Example 1 is that the first calcination temperature is 300°C, the second calcination temperature is 300°C, and the reduction treatment temperature is 200°C.

[0094] Example 8

[0095] The difference between Example 8 and Example 1 is that the first calcination temperature is 600°C, the second calcination temperature is 600°C, and the reduction treatment temperature is 600°C.

[0096] Comparative Example 1

[0097] The difference between Comparative Example 1 and Example 1 is that no prefabricated catalytic module is prepared, and the dispersion containing the silver source and the palladium source is directly impregnated and dispersed on SBA-15 to prepare a porous honeycomb catalytic coating module.

[0098] Comparative Example 2

[0099] The difference between Comparative Example 2 and Example 1 is that no manganese source, cerium source and zirconium source are added, and only TiCl4 is added, and a porous honeycomb catalytic coating module is obtained after the first drying and the first sintering.

[0100] Comparative Example 3

[0101] The difference between Comparative Example 3 and Example 4 is that no manganese source, cerium source and zirconium source are added, and only TiCl4 is added.

[0102] Comparative Example 4

[0103] The difference between Comparative Example 4 and Example 4 is that no manganese source and cerium source are added, only ZrO(NO3)2 and TiCl4 are added, and the molar ratio of Zr to Ti elements is 1:1.

[0104] Comparative Example 5

[0105] The difference between Comparative Example 5 and Example 4 is that no manganese source is added, and only Ce(NO3)3·6H2O, ZrO(NO3)2 and TiCl4 are added, and the molar ratio of Ce, Zr and Ti elements is 0.5:1:1.

[0106] Comparative Example 6

[0107] The difference between Comparative Example 6 and Example 1 is that no manganese source, cerium source and zirconium source are added, only TiCl4 is added, and the dispersion liquid used in the impregnation method does not contain silver nitrate, but only palladium nitrate.

[0108] Comparative Example 7

[0109] The difference between Comparative Example 7 and Example 4 is that no manganese source, cerium source and zirconium source are added, only TiCl4 is added, and the dispersion liquid used in the impregnation method does not contain palladium nitrate, but only silver nitrate.

[0110] Comparative Example 8

[0111] The difference between Comparative Example 8 and Example 4 is that the same molar amount of Cu(NO3)2 is used instead of Mn(NO3)2·6H2O.

[0112] Comparative Example 9

[0113] The difference between Comparative Example 9 and Example 4 is that the same molar amount of Mg(NO3)2 is used instead of Ce(NO3)3·6H2O.

[0114] Application Examples

[0115] The porous honeycomb catalytic coating modules prepared in Examples 1-8 and Comparative Examples 1-9 were respectively placed in the structural parts containing the porous plate electrode high-voltage power supply and the fan with the same parameters to form a circulation purification module, and tested in the same refrigerator freezer area. A certain concentration of durian odor was generated in the freezer area, and then the purification was turned on for a fixed time to test the odor purification effect; the odor degree was qualitatively judged by the same professional odorist, and the judgment standard was based on the odor intensity classification method, 0-odorless, 1-barely able to feel the odor, 2-very weak odor but able to distinguish its nature, 3-very easy to feel the odor, 4-strong odor, unbearable extremely strong odor; the test results are shown in Table 1 below.

[0116] Table 1

[0117]

[0118]

[0119] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0120] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A catalyst, characterized in that The catalyst comprises a composite carrier and Ag and Pd loaded on the composite carrier. The composite carrier comprises a mesoporous molecular sieve and a MnCeZrTi composite semiconductor material loaded on the mesoporous molecular sieve.

2. The catalyst according to claim 1, characterized in that The total mass of Mn, Ce, Zr and Ti elements in the MnCeZrTi composite semiconductor material is 0.5%-10% of the mass of the mesoporous molecular sieve; And / or, in the MnCeZrTi composite semiconductor material, the molar ratio of Mn, Ce, Zr and Ti is (0.01-1):(0.01-1):(0.1-2):

1.

3. The catalyst according to claim 1, characterized in that The mass of Ag is 0.1%-5% of the mass of the composite carrier; And / or, the mass of the Pd is 0.01%-0.5% of the mass of the composite carrier.

4. The catalyst according to claim 1, characterized in that The pore size of the mesoporous molecular sieve is 2nm-50nm; And / or, the mesoporous molecular sieve includes SBA-15.

5. A method for preparing the catalyst according to any one of claims 1 to 4, characterized in that: The steps include: The dispersion of citric acid is mixed with a manganese source, a cerium source, a zirconium source, a titanium source and a mesoporous molecular sieve to obtain a mixture, and the mixture is dried for the first time and calcined for the first time under a protective atmosphere to obtain a composite carrier; The dispersion containing the silver source and the palladium source is mixed with the composite carrier, and the catalyst is prepared through a second drying, a second calcination and a reduction treatment.

6. The method for preparing the catalyst according to claim 5, characterized in that: The molar ratio of citric acid in the citric acid dispersion to the Ti element in the titanium source is (0.05-0.5):1; And / or, in the mixture, the molar ratio of the Mn element in the manganese source, the Ce element in the cerium source, the Zr element in the zirconium source and the Ti element in the titanium source is (0.01-1):(0.01-1):(0.1-2):1; And / or, in the mixture, the total mass of the Mn element in the manganese source, the Ce element in the cerium source, the Zr element in the zirconium source and the Ti element in the titanium source is 0.5%-10% of the mass of the mesoporous molecular sieve; And / or, the first drying temperature is 60°C-180°C, and the time is 0.5h-5h; And / or, the protective atmosphere includes at least one of nitrogen and argon; And / or, the temperature of the first calcination is 300° C.-600° C., and the time is 0.5 h-5 h.

7. The method for preparing a catalyst according to claim 5, characterized in that: The mass of the Ag element in the silver source is 0.1%-5% of the mass of the composite carrier; and / or, the mass of the Pd element in the palladium source is 0.01%-0.5% of the mass of the composite support; And / or, the temperature of the second drying is 60°C-180°C, and the time is 0.5h-5h; And / or, the second calcination temperature is 300°C-600°C, and the time is 0.5h-5h; And / or, the reduction treatment temperature is 200° C.-600° C., the time is 0.1 h-5 h, and the reducing atmosphere includes hydrogen.

8. A catalytic module, comprising a porous substrate and a catalyst coating distributed on the surface of the porous substrate, characterized in that: The catalyst coating comprises the catalyst according to any one of claims 1 to 4.

9. A method for preparing a catalytic module as claimed in claim 8, characterized in that: The steps include: Mixing the citric acid dispersion with a manganese source, a cerium source, a zirconium source, a titanium source and a mesoporous molecular sieve to obtain a mixture; Placing the mixture on the surface of a porous substrate, drying it for the first time and calcining it for the first time under a protective atmosphere to obtain a prefabricated catalytic module; A dispersion containing a silver source and a palladium source is placed on the surface of the prefabricated catalytic module, and the catalytic module is obtained through a second drying, a second calcination and a reduction treatment.

10. The method for preparing a catalytic module according to claim 9, characterized in that: The mixture also includes a binder, the binder includes aluminum sol, and the mass of the binder is 2%-15% of the mass of the mesoporous molecular sieve; And / or, the porous substrate comprises a porous ceramic substrate; And / or, the mixture is placed on the surface of the porous substrate by vacuum coating; And / or, the method of placing the dispersion containing the silver source and the palladium source on the surface of the prefabricated catalytic module is selected from the impregnation method.

11. A gas purification system, characterized in that: Comprising the catalytic module as claimed in claim 8.

Citation Information

Patent Citations

  • Catalytic ozonation catalyst and preparation method thereof and method for treating toluene-containing waste gas by using catalytic ozonation catalyst

    CN110961153A

  • Catalyst suitable for low-temperature plasma and preparation method and application thereof

    CN115055204A

  • Catalyst and preparation method thereof, catalytic module and gas purification system

    CN116920919A

  • Catalyst for treating organic waste gas containing domestic oil fume and preparation method of catalyst

    CN117138830A

  • A generator