Method for carrying out iron ore reverse flotation by using combined collecting agent

The problems of high energy consumption and environmental pollution in the iron ore antiflotation process are solved by using a combination of Plulandosaccharide, calcium chloride, sodium oleate and dodecyl imidazoline in low alkalinity environments. , realizes efficient and environmentally friendly iron ore development and utilization, and reduces the energy consumption and environmental impact of the ore dressing process.

CN118874692APending Publication Date: 2024-11-01NORTHEASTERN UNIV CHINA

Patent Information

Application Number
CN202411157383.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing iron ore anti-flotation process has problems of high energy consumption, complex configuration and environmental pollution, especially in high alkali and high temperature conditions, which are difficult to effectively solve.

Method used

Using combined collectors in low alkalinity environments, including prurandosaccharide, calcium chloride, sodium oleate and dodecyl imidazoline, the high efficiency of iron ore is achieved through inhibitors and activators. Reverse flotation, reduce energy consumption and improve biodegradability.

Benefits of technology

It significantly reduces the energy consumption of the ore production process under normal temperature conditions, improves the development and utilization rate of iron ore resources, reduces environmental pollution, complies with the "dual carbon" goal, and has a simple configuration process and strong harvesting capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874692A_ABST
    Figure CN118874692A_ABST
Patent Text Reader

Abstract

A method for carrying out iron ore reverse flotation by using a combined collecting agent belongs to the field of mineral processing flotation, and comprises the following steps: grinding raw ore to obtain ore pulp with fixed grinding fineness; the ore pulp is subjected to tailing discarding in advance, and obtained magnetic separation concentrate is fed into a stirring barrel to adjust the concentration of the ore pulp; an inhibitor is added into the ore pulp and stirred, then an activating agent is added and stirred, then a combined collecting agent is added for full pulp mixing, then the ore pulp is fed into a flotation machine, inflation is started for roughing operation, and a roughing concentrate product and a roughing tailing product are obtained respectively; in the obtained roughing concentrate product, the combined collecting agent continues to be added for concentration operation, and iron concentrate is obtained; scavenging operation is conducted on the roughing tailings under the condition that no collecting agent is added, and flotation tailings are obtained. The combined collecting agent has the advantages of being high in collecting capacity and low in agent dosage, efficient flotation can be achieved in the alkalescent environment, and the bad influence on the environment due to the fact that agents are left in flotation return water is effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of mineral processing and flotation, and in particular relates to a method for reverse flotation of iron ore using a combined collector. Background Art

[0003] Flotation technology is one of the effective methods to treat low-grade, fine-grained and difficult-to-select iron ore, and is an effective way to improve the comprehensive utilization of my country's iron resources. Iron ore flotation is usually divided into positive flotation and reverse flotation processes. Among them, the reverse flotation process can be divided into two types: cationic collector reverse flotation and anionic collector reverse flotation. Although cationic collector reverse flotation has the advantages of simple reagent system and low temperature resistance, it is sensitive to ore slime reaction, high viscosity of foam products, and complex subsequent treatment; although anionic collectors can obtain products with higher indicators, they need to float in a strong alkaline environment, and the configuration temperature is too high (50-70°C), resulting in high energy consumption. With the increasing complexity of ore properties, as well as many factors such as the harsh flotation environment and high requirements for downstream smelting raw materials, higher requirements have been put forward for flotation reagents. For example, patent CN110479496B proposes a composite amphoteric collector for reverse flotation of iron ore and its application, which can effectively reduce the flotation temperature of ore and improve the stickiness and brittleness of flotation bubbles. However, the configuration of the agent is relatively complex and requires the use of multiple components in a mixed manner, which increases the complexity of the separation operation. Patent CN101912822A discloses a series of anionic and cationic collectors for iron ore flotation and their preparation methods. This method has the problem that the main agent remains unchanged and only part of the emulsifier is added for agent emulsification. This method cannot effectively solve the high-alkali and high-temperature flotation conditions that exist when the agent itself is used in the production process. Summary of the invention

[0004] In view of the deficiencies of the prior art, the technical problem to be solved by the present invention is to achieve the development and utilization of low-grade iron ore by reducing the energy consumption of mineral processing and thereby improve the self-sufficiency rate of iron ore resources, while ensuring the environmental protection and high efficiency of the production process. The present invention provides a method for realizing efficient reverse flotation of iron ore by using a combined collector in a low alkalinity flotation environment with a pulp pH of 7 to 9. The collector has excellent biodegradability and is less harmful to the environment. At the same time, after the collector is configured under heating conditions, its application under normal temperature conditions can greatly reduce the energy consumption in the mineral processing production process, which is in line with the background of the "dual carbon" goal.

[0005] In order to solve the above technical problems, the specific technical solutions of the present invention are as follows:

[0006] A method for reverse flotation of iron ore using a combined collector comprises the following steps:

[0007] (1) Grinding the raw ore to obtain a slurry with a fixed grinding fineness;

[0008] (2) feeding the ore pulp into a magnetic separator for pre-tailing, and feeding the magnetic concentrate obtained after tailing into a mixing tank to adjust the ore pulp concentration;

[0009] (3) adding a pullulan solution as an inhibitor to the slurry obtained in step (2) and stirring for a period of time to inhibit the floatability of iron minerals in the slurry, then adding an activator calcium chloride solution and stirring to activate the gangue minerals, and finally adding a combined collector solution to fully prepare the slurry;

[0010] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0011] (5) Adding a combined collector solution to the obtained roughing concentrate product to carry out a concentration operation to obtain an iron concentrate; and performing a scavenging operation on the roughing tailings without adding a collector to obtain a flotation tailings.

[0012] in:

[0013] In the step (1), the material fineness in the slurry is -0.038 mm, accounting for 40-70%.

[0014] In the step (2), the grade of the magnetic concentrate TFe obtained after tailings removal is 40-55%, and the slurry concentration after adjustment is 30-50%.

[0015] In the step (3), the pullulan solution is prepared by adding pullulan into water, stirring and dissolving the solution, with a mass concentration of 0.1-1%.

[0016] In the step (3), the preparation method of the calcium chloride solution is: adding calcium chloride into water, stirring and dissolving the solution, and the mass concentration is 0.1-1%.

[0017] In the steps (3) and (5), the preparation method of the combined collector solution is: sodium oleate and dodecyl imidazoline are mixed in a mass ratio of (3-10):1, and then added into water at a temperature of 30-60°C for stirring and dissolving to obtain a mass concentration of 0.1-1%.

[0018] In the step (3), the ore slurry is stirred for 3 to 5 minutes after the inhibitor is added, and stirred for 3 to 5 minutes after the activator is added.

[0019] In the step (3), the amount of the inhibitor is 200 to 1000 g·t -1 , the amount of activator is 100~500g·t -1 The amount of collector is 50~500g·t -1 .

[0020] In the step (5), the rough concentrate is subjected to a first concentration operation, and the amount of collector used is 20 to 100 g·t -1 .

[0021] In the step (5), the roughing tailings are subjected to three scavenging operations, and no reagents are added during the scavenging process.

[0022] In the step (5), the tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection.

[0023] In the step (5), the TFe content of the iron ore concentrate is ≥ 65%.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention adopts pullulan as an inhibitor for reverse flotation of iron ore. The inhibitor has good water solubility and a simple preparation process.

[0026] 2. In the combined collector used in the present invention, dodecyl imidazoline has good water solubility and has certain collecting properties and strong foaming properties. When mixed with sodium oleate, the collecting property of sodium oleate is improved by molecular association, while significantly reducing the amount of sodium oleate used, the application temperature, and the alkalinity of the application environment.

[0027] 3. The combined agent of the present invention has the advantages of strong collecting ability and low agent dosage compared with traditional fatty acid collectors during use, further realizing cost reduction and efficiency improvement in the process of iron ore development and utilization. At the same time, since dodecyl imidazoline has excellent biodegradability and can achieve efficient flotation in a weakly alkaline environment, it reduces the difficulty of mineral processing wastewater treatment and effectively reduces the adverse impact of the agent residue in the flotation return water on the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 A process flow chart of the invention for reverse flotation of iron ore using a combined collector. DETAILED DESCRIPTION

[0029] In order to further illustrate the technical means and effects of the present invention to achieve the expected effects, the present invention will be described in detail below in conjunction with the accompanying drawings and embodiments of the specification. Obviously, the embodiments described are only some implementation cases of the present invention. Therefore, it should be noted that the scope of protection of the present invention is not limited to the following specific embodiments, and the embodiments obtained in the art without significant creative improvements on the basis of the present invention belong to the protection scope of the present invention.

[0030] In the embodiment of the present invention, the preparation method of the inhibitor pullulan solution is: adding pullulan into water, stirring and dissolving the solution.

[0031] In the embodiment of the present invention, the preparation method of the activator calcium chloride solution is: adding calcium chloride into water, stirring and dissolving the solution.

[0032] In the embodiment of the present invention, the preparation method of the combined collector solution is: sodium oleate and dodecyl imidazoline are mixed in a ratio of (3-10):1, and then added into water at a temperature of 30-60°C for stirring and dissolving.

[0033] Example 1

[0034] A method for reverse flotation of iron ore using a combined collector, the process flow chart of which is as follows: Figure 1 As shown, the specific steps include:

[0035] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 45%.

[0036] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 41.54% in TFe grade, 16.25% in SiO2, and 6.19% in F content. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel, and the ore pulp concentration is adjusted to 30%; sodium oleate and dodecyl imidazoline are mixed in a ratio of 5:1, and then added into water at a temperature of 40°C for stirring and dissolving to obtain a combined collector solution;

[0037] (3) Add 300 g / t of pullulan solution with a mass concentration of 0.3% to the slurry obtained in step (2). -1 , stirring for 3 minutes to suppress the floatability of iron minerals, and then adding 0.2% calcium chloride solution in an amount of 150g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding a combined collector solution with a mass concentration of 0.1% and a dosage of 360 g·t -1 , fully prepare the slurry;

[0038] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0039] (5) Add 100 g·t of combined collector solution with a mass concentration of 0.1% to the obtained rough concentrate product. -1, start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0040] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 1.

[0041] Table 1 Index of products obtained in Example 1

[0042] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.83 55.97 Flotation tailings 10.66 44.03 total 41.54 100

[0043] Example 2

[0044] A method for reverse flotation of iron ore using a combined collector comprises the following steps:

[0045] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 50%.

[0046] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 44.82% TFe, 24.87% SiO2 and 6.08% F. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel, and the ore pulp concentration is adjusted to 35%; sodium oleate and dodecyl imidazoline are mixed in a ratio of 3:1, and then added into water at a temperature of 30°C for stirring and dissolving to obtain a combined collector solution;

[0047] (3) Add 400 g·t of pullulan solution with a mass concentration of 0.1% to the slurry obtained in step (2); -1 , stirring for 4 minutes to suppress the floatability of iron minerals, and then adding 0.3% calcium chloride solution in an amount of 100 g·t -1 , stirring for 3 minutes to activate the gangue minerals, and then adding a combined collector solution with a mass concentration of 0.4% in an amount of 340 g·t -1 , fully prepare the slurry;

[0048] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0049] (5) Add 150 g·t of combined collector solution with a mass concentration of 0.4% to the obtained rough concentrate product. -1, start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0050] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 2.

[0051] Table 2 Index of products obtained in Example 2

[0052] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.73 62.24 Flotation tailings 10.35 37.76 total 44.82 100

[0053] Example 3

[0054] A method for reverse flotation of iron ore using a combined collector comprises the following steps:

[0055] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 55%.

[0056] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 46.2% in TFe grade, 20.93% in SiO2, and 1.8% in F content. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel, and the ore pulp concentration is adjusted to 40%; sodium oleate and dodecyl imidazoline are mixed in a ratio of 8:1, and then added into water at a temperature of 55°C for stirring and dissolving to obtain a combined collector solution;

[0057] (3) Add 450 g·t of pullulan solution with a mass concentration of 0.5% to the slurry obtained in step (2). -1 , stirring for 5 minutes to suppress the floatability of iron minerals, and then adding 0.5% calcium chloride solution in an amount of 200g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding a combined collector solution with a mass concentration of 0.7% and a dosage of 300 g·t -1 , fully prepare the slurry;

[0058] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0059] (5) Add 0.7% combined collector solution to the rough concentrate product in an amount of 50 g·t -1, start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0060] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 3.

[0061] Table 3 Index of products obtained in Example 3

[0062] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.07 63.92 Flotation tailings 12.77 36.08 total 46.2 100

[0063] Example 4

[0064] A method for reverse flotation of iron ore using a combined collector comprises the following steps:

[0065] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 60%.

[0066] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 49.54% in TFe grade, 23.44% in SiO2, and 4.61% in F content. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel, and the ore pulp concentration is adjusted to 30%; sodium oleate and dodecyl imidazoline are mixed in a ratio of 4:1, and then added into water at a temperature of 40°C for stirring and dissolving to obtain a combined collector solution;

[0067] (3) Add 580 g·t of pullulan solution with a mass concentration of 0.2% to the slurry obtained in step (2). -1 , stirring for 3 minutes to suppress the floatability of iron minerals, and then adding 0.2% calcium chloride solution in an amount of 100g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding a combined collector solution with a mass concentration of 1% and a dosage of 400g·t -1 , fully prepare the slurry;

[0068] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0069] (5) Add 60 g·t of combined collector solution with a mass concentration of 1% to the obtained rough concentrate product. -1, start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0070] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 4.

[0071] Table 4 Product indicators of Example 4

[0072] Product Name TFe grade / % Recovery rate / % Iron Concentrate 66.68 67.46 Flotation tailings 14.01 32.54 total 49.54 100

[0073] Example 5

[0074] A method for reverse flotation of iron ore using a combined collector comprises the following steps:

[0075] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 65%.

[0076] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 50.67% in TFe grade, 15.75% in SiO2, and 0.22% in F content. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel, and the ore pulp concentration is adjusted to 45%; sodium oleate and dodecyl imidazoline are mixed in a ratio of 3:1, and then added into water at a temperature of 30°C for stirring and dissolving to obtain a combined collector solution;

[0077] (3) Add 650 g·t of pullulan solution with a mass concentration of 0.4% to the slurry obtained in step (2). -1 , stirring for 3.5 min to suppress the floatability of iron minerals, and then adding 0.1% calcium chloride solution in an amount of 300 g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding a combined collector solution with a mass concentration of 0.6% and a dosage of 200 g·t -1 , fully prepare the slurry;

[0078] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0079] (5) Add 0.6% combined collector solution to the rough concentrate product in an amount of 50 g·t -1, start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0080] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 5.

[0081] Table 5 Index of products obtained in Example 5

[0082] Product Name TFe grade / % Recovery rate / % Iron Concentrate 67.73 69.15 Flotation tailings 12.43 30.85 total 50.67 100

[0083] Example 6

[0084] A method for reverse flotation of iron ore using a combined collector comprises the following steps:

[0085] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 70%.

[0086] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 46.86% in TFe grade, 18.35% in SiO2, and 2.6% in F content. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel, and the ore pulp concentration is adjusted to 50%; sodium oleate and dodecyl imidazoline are mixed in a ratio of 5:1, and then added into water at a temperature of 45°C for stirring and dissolving to obtain a combined collector solution;

[0087] (3) Add 370 g·t of pullulan solution with a mass concentration of 1% to the slurry obtained in step (2). -1 , stirred for 4 minutes to suppress the floatability of iron minerals, and then added 0.5% calcium chloride solution in an amount of 250 g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding a combined collector solution with a mass concentration of 0.3% and a dosage of 260 g·t -1 , fully prepare the slurry;

[0088] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0089] (5) Add 80 g·t of combined collector solution with a mass concentration of 0.3% to the obtained rough concentrate product. -1, start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0090] Among them, the tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 6.

[0091] Table 6 Index of the product obtained in Example 6

[0092] Product Name TFe grade / % Recovery rate / % Iron Concentrate 65.9 67.56 Flotation tailings 7.21 32.44 total 46.86 100

[0093] Comparative Example 1

[0094] A method for reverse flotation of iron ore, comprising the following steps:

[0095] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 50%.

[0096] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 44.82% TFe, 24.87% SiO2 and 6.08% F. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz and fluorite. The magnetic concentrate is fed into a mixing barrel and the ore pulp concentration is adjusted to 35%;

[0097] (3) Add 400 g·t of pullulan solution with a mass concentration of 0.1% to the slurry obtained in step (2); -1 , stirring for 5 minutes to suppress the floatability of iron minerals, and then adding 0.3% calcium chloride solution in an amount of 100 g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding 0.4% sodium oleate solution in an amount of 800 g·t -1 , fully prepare the slurry;

[0098] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0099] (5) Add 0.4% sodium oleate solution to the rough concentrate product in an amount of 400 g·t -1 , start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0100] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 7. Compared with Example 2, the use of the combined collector can not only obtain better flotation indicators, but also reduce its dosage.

[0101] Table 7 Comparative Example 1 Product Index

[0102] Product Name TFe grade / % Recovery rate / % Iron Concentrate 64.51 55.45 Flotation tailings 20.31 44.55 total 44.82 100

[0103] Comparative Example 2

[0104] A method for reverse flotation of iron ore, comprising the following steps:

[0105] (1) A certain iron ore was ground to obtain a slurry with a fixed grinding fineness of -0.038 mm and a proportion of 60%.

[0106] (2) The ore pulp is fed into a magnetic separator for pre-tailing. The magnetic concentrate obtained after tailing is 49.54% in TFe grade, 23.44% in SiO2 content, and 4.61% in F content. The main metal mineral components in the ore are hematite and magnetite, and the non-metallic gangue minerals are mainly quartz, fluorite, etc. The magnetic concentrate is fed into a mixing barrel and the ore pulp concentration is adjusted to 30%;

[0107] (3) Add 580 g·t of pullulan solution with a mass concentration of 0.2% to the slurry obtained in step (2). -1 , stirring for 3 minutes to suppress the floatability of iron minerals, and then adding 0.2% calcium chloride solution in an amount of 100g·t -1 , stirring for 3 minutes to activate the gangue minerals, and finally adding 1% sodium oleate solution in an amount of 1000 g·t -1 , fully prepare the slurry;

[0108] (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively;

[0109] (5) Add 1% sodium oleate solution to the rough concentrate product in an amount of 500 g / t -1 , start aeration to carry out concentration operation to obtain iron concentrate; carry out three scavenging operations on the roughing tailings without adding collector to obtain flotation tailings;

[0110] The tailings obtained from the cleaning operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (3) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection. The TFe grade and recovery rate of the obtained iron concentrate and flotation tailings are shown in Table 8. Compared with Example 4, the use of the combined collector can not only obtain better flotation indicators, but also reduce its dosage.

[0111] Table 8 Product indexes of comparative example 2

[0112]

[0113]

[0114] The above are only preferred examples of the present invention and cannot limit the scope of implementation of the present invention. That is, all embodiments obtained in the art without significant creative improvements based on the present invention belong to the protection scope of the present invention.

Claims

1. A method for reverse flotation of iron ore using a combined collector, characterized in that: The specific steps include: (1) Grinding the raw ore to obtain a slurry with a fixed grinding fineness; (2) feeding the ore pulp into a magnetic separator for pre-tailing, and feeding the magnetic concentrate obtained after tailing into a mixing tank to adjust the ore pulp concentration; (3) adding a pullulan solution as an inhibitor to the slurry obtained in step (2) and stirring for a period of time to inhibit the floatability of iron minerals in the slurry, then adding an activator calcium chloride solution and stirring to activate the gangue minerals, and finally adding a combined collector solution to fully prepare the slurry; (4) feeding the slurry after the reagent is acted upon into a flotation machine and starting aeration to perform a roughing operation, thereby obtaining a roughing concentrate product and a roughing tailings product respectively; (5) adding a combined collector solution to the obtained roughing concentrate product to perform a concentration operation to obtain an iron concentrate; and performing a scavenging operation on the roughing tailings without adding a collector to obtain a flotation tailings; The tailings obtained from the concentration operation are combined with the concentrate obtained from the first scavenging operation and returned to the roughing operation in step (4) for reselection; the concentrate obtained from the second scavenging operation is returned to the first scavenging operation process for reselection; and the concentrate obtained from the third scavenging operation is returned to the second scavenging operation process for reselection.

2. A method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In step (1), the material fineness in the slurry is -0.038 mm, accounting for 40 to 70%.

3. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (2), the grade of the magnetic concentrate TFe obtained after tailings removal is 40-55%, and the slurry concentration after adjustment is 30-50%.

4. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (3), the pullulan solution is prepared by adding pullulan into water, stirring and dissolving the solution, with a mass concentration of 0.1-1%.

5. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (3), the preparation method of the calcium chloride solution is: adding calcium chloride into water, stirring and dissolving the solution, and the mass concentration is 0.1-1%.

6. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the steps (3) and (5), the preparation method of the combined collector solution is: sodium oleate and dodecyl imidazoline are mixed in a mass ratio of (3-10):1, and then added into water at a temperature of 30-60°C for stirring and dissolving to obtain a mass concentration of 0.1-1%.

7. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (3), the ore slurry is stirred for 3 to 5 minutes after the inhibitor is added, and stirred for 3 to 5 minutes after the activator is added.

8. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (3), the amount of the inhibitor is 200 to 1000 g·t -1 , the amount of activator is 100~500g·t -1 The amount of collector is 50~500g·t -1 .

9. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (5), the rough concentrate is subjected to a first concentration operation, and the amount of collector used is 20 to 100 g·t -1 The roughing tailings are swept three times, and no reagents are added during the sweeping process.

10. The method for reverse flotation of iron ore using a combined collector according to claim 1, characterized in that: In the step (5), the TFe content of the iron ore concentrate is ≥ 65%.

Citation Information

Patent Citations

  • Mixture of an amine alkoxylate ester and a quaternary ammonium compound as a collector for minerals containing silicate

    CN102112235A

  • Depressants for mineral ore flotation

    CN104822460A

  • Cationic flotation collecting agent and application thereof

    CN111330742A

  • Application of low-temperature inhibitor pullulan in iron ore reverse flotation and application method

    CN115254441A

Cited By

  • Combined collecting agent for low-temperature type iron ore flotation desilicication and application of combined collecting agent

    CN119972362A

  • Low-temperature type iron ore flotation desilication combined collector and application thereof

    CN119972362B