Method for preparing low-oxygen high-purity titanium powder by utilizing recycled high-purity titanium residual target

By using a hydrogenation-dehydrogenation process to process high-purity titanium residue under inert gas protection, the problem of high cost in recycling and reusing high-purity titanium residue has been solved, and the efficient preparation of low-oxygen high-purity titanium powder has been achieved, improving production efficiency and product quality.

CN118875290APending Publication Date: 2024-11-01宁波创润新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410930301.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The recycling and reuse of high-purity titanium targets in existing technologies relies on electron beam vacuum remelting technology, which results in high initial investment and operating costs and a slow process, making it difficult to meet the demand for efficient and low-cost high-purity titanium powder production.

Method used

The hydrogenation and dehydrogenation process is adopted, including acid washing, water washing, vacuum drying, hydrogenation treatment, crushing and screening, and dehydrogenation treatment. All processes are carried out under inert gas protection. Temperature and pressure are controlled in multiple stages to ensure the preparation of low-oxygen, high-purity titanium powder.

Benefits of technology

This reduced production costs, improved production efficiency, and enabled the production of low-oxygen, high-purity titanium powder to meet the needs of high-end users, thereby enhancing market competitiveness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of metal recovery, in particular to a method for preparing low-oxygen high-purity titanium powder through recycled high-purity titanium residual targets, and the method for preparing the low-oxygen high-purity titanium powder through the recycled high-purity titanium residual targets comprises the steps that firstly, the recycled high-purity titanium residual targets are sequentially subjected to acid pickling treatment, water washing treatment and vacuum drying treatment; 2, the titanium residual target obtained after vacuum drying treatment is subjected to hydrotreating, and a titanium hydride residual target is obtained; 3, under protection of inert gas, the titanium hydride residual target is subjected to first crushing treatment, and the titanium hydride residual target with the first size is obtained; 4, under the protection of inert gas, the titanium hydride residual target with the first size is subjected to second crushing treatment, and titanium hydride powder with the second size is obtained; 5, under the protection of inert gas, the titanium hydride powder with the second size is subjected to dehydrogenation treatment, and low-oxygen high-purity dehydrogenated titanium with the second size is obtained; all procedures of hydrogenation and dehydrogenation are operated under the protection of inert gas, so that the increment of powder gas elements in the recovery process is controlled within 100 ppm, operation is performed in a closed environment, and the risk of introducing foreign matters in the process is eliminated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal recovery, and in particular to a method for preparing low-oxygen high-purity titanium powder by utilizing recovered high-purity titanium residual targets. Background Art

[0002] In the current production and application of high-purity titanium materials, the efficient recycling of waste resources has always been the focus of the industry. Traditionally, the recycling and reuse of high-purity titanium residual targets mainly relies on electron beam vacuum remelting technology. This process uses high-energy electron beams to directly irradiate the residual targets in a high vacuum environment to achieve precise melting and recasting of materials, which can remove impurities to a large extent and obtain high-purity titanium alloys.

[0003] However, the use of electron beam vacuum remelting technology requires complex vacuum equipment and high-energy electron beam generating devices, which leads to relatively high initial investment and operating costs. Compared with other welding or smelting technologies, the electron beam vacuum remelting technology is also relatively slow. In view of the limitations of the existing technology, the present invention provides an innovative hydrogenation and dehydrogenation process route, which is a technical solution specifically used for the recovery and reuse of high-purity titanium residual targets, thereby reducing the operating and investment costs of enterprises and increasing high value-added titanium powder products. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target in view of the deficiencies in the prior art.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target, comprising the following steps:

[0007] Step 1: The recovered high-purity titanium residual target is sequentially subjected to pickling treatment, water washing treatment, and vacuum drying treatment;

[0008] Step 2, hydrogenating the titanium residual target after vacuum drying to obtain a hydride titanium residual target;

[0009] Step 3: Under the protection of an inert gas, the titanium hydride residual target is subjected to a first crushing process to obtain a titanium hydride residual target having a first size;

[0010] Step 4: Under the protection of an inert gas, the titanium hydride residual target having the first size is subjected to a second crushing and screening process to obtain titanium hydride powder having a second size;

[0011] Step 5: Under the protection of an inert gas, the titanium hydride powder having the second size is subjected to a dehydrogenation treatment to obtain low-oxygen high-purity dehydrogenated titanium having the second size;

[0012] The hydrogenation treatment includes: a first heating stage, a first heat preservation stage, a second heating stage, a second heat preservation stage, a cooling stage, a hydrogenation stage, and a first cooling stage.

[0013] The dehydrogenation treatment includes, in sequence: a third heating stage, a third heat preservation stage, a fourth heating stage, a fourth heat preservation stage, a fifth heating stage, a fifth heat preservation stage, a sixth heating stage, a sixth heat preservation stage, a seventh heating stage, a seventh heat preservation stage, an eighth heating stage, an eighth heat preservation stage, and a second cooling stage;

[0014] The first size is larger than the second size, and the second size is larger than the third size.

[0015] Preferably, it also includes:

[0016] Step 0: Process the recovered high-purity titanium residual target into a strip-shaped titanium residual target of 5 mm×50 mm.

[0017] Preferably, it also includes:

[0018] Step 6: performing a third crushing on the dehydrogenated titanium with the second size to obtain low-oxygen high-purity dehydrogenated titanium with the third size;

[0019] Step 7, screening the dehydrogenated titanium with the third size to obtain low-oxygen high-purity dehydrogenated titanium powder;

[0020] Step 8, weighing and packaging the low-oxygen high-purity dehydrogenated titanium powder in sequence to obtain low-oxygen high-purity titanium powder;

[0021] Wherein, steps six to eight are all carried out under the protection of inert gas.

[0022] Preferably, the pickling treatment comprises: pickling the titanium residual target with a mixed solution of nitric acid and hydrofluoric acid;

[0023] Among them, the volume ratio of nitric acid to hydrofluoric acid is (1-3):(4-6).

[0024] Preferably, the heating and drying temperature of the vacuum heating and drying treatment is 90°C to 150°C.

[0025] Preferably, the first heating stage is to heat the temperature to 250°C, and the insulation time of the first insulation stage is 2h;

[0026] The second heating stage is to heat up to 750℃-800℃, and the insulation time of the second insulation stage is 4h;

[0027] The temperature in the cooling stage is lowered to 550°C, and the temperature in the hydrogenation stage is 500°C to 650°C.

[0028] Preferably, the third heating stage is to heat the temperature to 250°C, and the insulation time of the third insulation stage is 2h;

[0029] The fourth heating stage is to heat the temperature to 400°C, and the fourth insulation stage has an insulation time of 1h;

[0030] The fifth heating stage is to heat the temperature to 500°C, and the insulation time of the fifth insulation stage is 2h;

[0031] The sixth heating stage is to heat the temperature to 550°C, and the sixth heat preservation stage is to keep the temperature for 2h;

[0032] The seventh heating stage is to heat the temperature to 600°C, and the seventh heat preservation stage has a heat preservation time of 2h;

[0033] The eighth heating stage is to heat the temperature to 650° C., and the eighth keeping temperature stage is to keep the temperature until the dehydrogenation is completed.

[0034] Preferably, the inert gas is argon.

[0035] Preferably, the internal online oxygen content of the equipment used in the second crushing treatment and the third crushing treatment is not higher than 1000 ppm.

[0036] Preferably, the vacuum pressure of the vacuum drying process is no higher than 20Pa.

[0037] The present invention adopts the above technical solution, and has the following technical effects compared with the prior art:

[0038] The material transfer process in the hydrogenation and dehydrogenation process of the present invention uses an inert gas airtight protection for the material receiving tank, and each hydrogenation and dehydrogenation process is performed under the protection of the inert gas, so that the incremental content of the powder gas element in the recovery process is controlled within 100ppm, and the process is performed in a closed environment, eliminating the risk of introducing foreign matter in the process, thereby preparing low-oxygen high-purity titanium powder to meet the needs of high-end users. The technical solution of the present invention can also effectively improve production efficiency and product quality, and also obtain a broader profit margin and stronger market competitiveness due to the degree of cost reduction. DETAILED DESCRIPTION

[0039] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0041] The following specific examples further illustrate the present invention but are not intended to limit the present invention.

[0042] Example 1

[0043] This embodiment provides a method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target, the steps comprising:

[0044] Step 1, soaking the recovered high-purity titanium residual target in a nitric acid and hydrofluoric acid mixed solution with a volume ratio of 2:5 to carry out pickling treatment on the titanium residual target, soaking the recovered high-purity titanium residual target in the nitric acid and hydrofluoric acid mixed solution for 12 hours and then taking it out, washing it with water twice after taking it out, and placing the titanium residual target in a vacuum drying box for vacuum drying after the washing treatment is completed;

[0045] The heating and drying temperature of the vacuum heating and drying process is 90°C, and the vacuum pressure of the vacuum drying process is not higher than 20Pa;

[0046] Step 2, hydrogenating the titanium residual target after vacuum drying to obtain a hydride titanium residual target;

[0047] The hydrogenation treatment includes the following steps: the first heating stage is heating up to 250°C and holding time is 2h; the second heating stage is heating up to 750°C and holding time is 4h; the second cooling stage is cooling down to 550°C and hydrogen is started; the temperature of the hydrogenation stage is controlled at 500°C to obtain a titanium hydride residual target;

[0048] Step 3: Under the protection of an inert gas, a medium crusher is used to crush the titanium hydride residual target into 5 mm particles to obtain a titanium hydride residual target having a first size;

[0049] Step 4: Under the protection of inert gas, the material receiving tank storing the titanium hydride residual target of the first size is connected to the feed port of the airflow pulverizing classifier, and argon gas is used for replacement, so that the online oxygen content of the system in the airflow pulverizing classifier is ≤1000ppm, and then the pulverizing and collection are performed to obtain titanium hydride powder of the second size;

[0050] Step 5, connect the vacuum glove box to the dehydrogenation furnace, use argon gas to replace the vacuum glove box, so that the online oxygen content of the vacuum glove box system is ≤500ppm, under the protection of argon gas, place the titanium hydride powder of the second size in the dehydrogenation furnace, evacuate the dehydrogenation furnace until the dehydrogenation is completed, and perform the dehydrogenation furnace in sequence, heating to 250°C for 2h, heating to 400°C for 1h, heating to 500°C for 2h, heating to 550°C for 2h, heating to 600°C for 2h, heating to 650°C until the vacuum pressure in the dehydrogenation furnace is less than 10Pa for 1h, and the dehydrogenation treatment is completed to obtain low-oxygen and high-purity dehydrogenated titanium of the second size;

[0051] Step 6: Replace the impact mill classifier with argon gas so that the online oxygen content of the equipment is ≤1000ppm during operation, and use the impact mill classifier to perform a third crushing on the dehydrogenated titanium with the second size to obtain low-oxygen and high-purity dehydrogenated titanium with the third size;

[0052] Step 7: Replace the ultrasonic vacuum vibrating screen with argon gas so that the online oxygen content of the equipment is ≤500ppm during operation, and screen the low-oxygen and high-purity dehydrogenated titanium with the third size through different sieves to obtain low-oxygen and high-purity dehydrogenated titanium powder;

[0053] Step 8, after replacing the vacuum glove box with argon gas so that the online oxygen content of the equipment during operation is ≤500ppm, the low-oxygen high-purity dehydrogenated titanium powder is weighed and packaged in sequence to obtain low-oxygen high-purity titanium powder;

[0054] Wherein, steps 6 to 8 are all carried out under the protection of inert gas;

[0055] The first size is larger than the second size, and the second size is larger than the third size.

[0056] Example 2

[0057] This embodiment provides a method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target, the steps comprising:

[0058] Step 1, soaking the recovered high-purity titanium residual target in a mixed solution of nitric acid and hydrofluoric acid with a volume ratio of 2:5 to carry out pickling treatment on the titanium residual target, soaking the recovered high-purity titanium residual target in the mixed solution of nitric acid and hydrofluoric acid for 24 hours and then taking it out, washing it with water three times after taking it out, and placing the titanium residual target in a vacuum drying box for vacuum drying after the washing treatment is completed;

[0059] The heating and drying temperature of the vacuum heating and drying process is 150°C, and the vacuum pressure of the vacuum drying process is not higher than 20Pa;

[0060] Step 2, hydrogenating the titanium residual target after vacuum drying to obtain a hydride titanium residual target;

[0061] The hydrogenation treatment includes the following steps: the first heating stage is heated to 250°C and kept for 2 hours; the second heating stage is heated to 800°C and kept for 4 hours; the second cooling stage is cooled to 550°C and hydrogen is passed; the temperature of the hydrogenation stage is controlled at 650°C to obtain a hydrogenated titanium residual target;

[0062] Step 3: Under the protection of an inert gas, a medium crusher is used to crush the titanium hydride residual target into 1 mm particles to obtain a titanium hydride residual target having a first size;

[0063] Step 4: Under the protection of inert gas, the material receiving tank storing the titanium hydride residual target of the first size is connected to the feed port of the airflow pulverizing classifier, and argon gas is used for replacement, so that the online oxygen content of the system in the airflow pulverizing classifier is ≤1000ppm for pulverization and collection, and titanium hydride powder of the second size is obtained;

[0064] Step 5, connect the vacuum glove box to the dehydrogenation furnace, use argon gas to replace the vacuum glove box, so that the online oxygen content of the vacuum glove box system is ≤500ppm, under the protection of argon gas, place the titanium hydride powder of the second size in the dehydrogenation furnace, evacuate the dehydrogenation furnace until the dehydrogenation is completed, and perform the dehydrogenation furnace in sequence, heating to 250°C for 2h, heating to 400°C for 1h, heating to 500°C for 2h, heating to 550°C for 2h, heating to 600°C for 2h, heating to 650°C until the vacuum pressure in the dehydrogenation furnace is less than 10Pa for 2h, and the dehydrogenation treatment is completed to obtain low-oxygen and high-purity dehydrogenated titanium of the second size;

[0065] Step 6: Replace the impact mill classifier with argon gas so that the online oxygen content of the equipment is ≤1000ppm during operation, and use the impact mill classifier to perform a third crushing on the dehydrogenated titanium with the second size to obtain low-oxygen and high-purity dehydrogenated titanium with the third size;

[0066] Step 7: Replace the ultrasonic vacuum vibrating screen with argon gas so that the online oxygen content of the equipment is ≤500ppm during operation, and screen the low-oxygen and high-purity dehydrogenated titanium with the third size through different sieves to obtain low-oxygen and high-purity dehydrogenated titanium powder;

[0067] Step 8, replacing the vacuum glove box with argon gas so that the online oxygen content of the equipment during operation is ≤500ppm, weighing and packaging the low-oxygen high-purity dehydrogenated titanium powder in turn to obtain low-oxygen high-purity titanium powder;

[0068] Wherein, steps 6 to 8 are all carried out under the protection of inert gas;

[0069] The first size is larger than the second size, and the second size is larger than the third size.

[0070] As a preferred implementation mode, in step zero, the recovered high-purity titanium residual target is processed into a strip-shaped titanium residual target of 5 mm×50 mm.

[0071] The material transfer process in the hydrogenation and dehydrogenation process of the present invention uses an inert gas airtight protection for the material receiving tank, and each hydrogenation and dehydrogenation process is performed under the protection of the inert gas, so that the incremental content of the powder gas element in the recovery process is controlled within 100ppm, and the process is performed in a closed environment, eliminating the risk of introducing foreign matter in the process, thereby preparing low-oxygen high-purity titanium powder to meet the needs of high-end users. The technical solution of the present invention can also effectively improve production efficiency and product quality, and also obtain a broader profit margin and stronger market competitiveness due to the degree of cost reduction.

[0072] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target, It is characterized in that the steps include: Step 1, sequentially subjecting the recovered high-purity titanium residual target to acid washing, water washing, and vacuum drying; Step 2, hydrogenating the titanium residual target after vacuum drying to obtain a hydride titanium residual target; Step 3: Under the protection of an inert gas, the titanium hydride residual target is subjected to a first crushing process to obtain a titanium hydride residual target having a first size; Step 4: Under the protection of an inert gas, the titanium hydride residual target having the first size is subjected to a second crushing process to obtain titanium hydride powder having a second size; Step 5: Under the protection of an inert gas, the titanium hydride powder having the second size is subjected to a dehydrogenation treatment to obtain low-oxygen high-purity dehydrogenated titanium having the second size; The hydrogenation treatment includes, in sequence: a first heating stage, a first heat preservation stage, a second heating stage, a second heat preservation stage, a cooling stage, a hydrogenation stage, and a first cooling stage; The dehydrogenation treatment includes, in sequence: a third heating stage, a third heat preservation stage, a fourth heating stage, a fourth heat preservation stage, a fifth heating stage, a fifth heat preservation stage, a sixth heating stage, a sixth heat preservation stage, a seventh heating stage, a seventh heat preservation stage, an eighth heating stage, an eighth heat preservation stage, and a second cooling stage; The first size is larger than the second size, and the second size is larger than the third size.

2. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that Also includes: Step 0: Process the recovered high-purity titanium residual target into a strip-shaped titanium residual target of 5 mm×50 mm.

3. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that Also includes: Step 6: performing a third crushing on the dehydrogenated titanium with the second size to obtain low-oxygen high-purity dehydrogenated titanium with the third size; Step 7, screening the dehydrogenated titanium with the third size to obtain low-oxygen high-purity dehydrogenated titanium powder; Step 8, weighing and packaging the low-oxygen high-purity dehydrogenated titanium powder in sequence to obtain low-oxygen high-purity titanium powder; Wherein, steps six to eight are all carried out under the protection of inert gas.

4. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The pickling treatment comprises: pickling the titanium residual target with a mixed solution of nitric acid and hydrofluoric acid; Wherein, the volume ratio of the nitric acid to the hydrofluoric acid is (1-3):(4-6).

5. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The heating and drying temperature of the vacuum heating and drying process is 90°C to 150°C.

6. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The first heating stage is to heat the temperature to 250°C, and the first heat preservation stage is to keep the temperature for 2 hours; The second heating stage is to heat the temperature to 750°C-800°C, and the second heat preservation stage is to keep the temperature for 4 hours; The temperature in the cooling stage is lowered to 550°C, and the temperature in the hydrogenation stage is 500°C to 650°C.

7. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The third heating stage is to heat the temperature to 250°C, and the insulation time of the third insulation stage is 2h; The fourth heating stage is to heat the temperature to 400° C., and the fourth heat preservation stage is to keep the temperature for 1 hour; The fifth heating stage is to heat the temperature to 500° C., and the insulation time of the fifth insulation stage is 2 hours; The sixth heating stage is to heat the temperature to 550° C., and the insulation time of the sixth insulation stage is 2 hours; The seventh heating stage is to heat the temperature to 600° C., and the seventh insulation stage is for 2 hours; the eighth heating stage is to heat the temperature to 650° C., and the eighth insulation stage is for insulation until the dehydrogenation is completed.

8. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The inert gas is argon.

9. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The internal online oxygen content of the equipment used in the second crushing process and the third crushing process is no higher than 1000 ppm.

10. The method for preparing low-oxygen high-purity titanium powder by recycling high-purity titanium residual target according to claim 1, It is characterized in that The vacuum pressure of the vacuum drying process is not higher than 20Pa.