Method for recovering magnesium and phosphorus resources from phosphorite
Through the synergistic effect of the countercurrent spray absorption tower process and zinc sulfate and disodium ethylenediaminetetraacetic acid, the leaching rate of magnesium and phosphorus in phosphate ore is improved, and the problem of high cost of magnesium demagnesium in the existing technology is solved. Efficient SO2 removal and resource utilization are achieved, reducing production costs.
Patent Information
- Application Number
- CN202410887016.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-03
AI Technical Summary
The prior art has high cost and low efficiency in the demagnesium process of magnesium in phosphate ores, especially the excessive use of sulfuric acid and the excessive addition of disodium ethylenediaminetetraacetic acid, resulting in high economic costs.
Using counter-current spray absorption tower process, phosphate ore, zinc sulfate and disodium ethylenediaminetetraacetic acid grinding are prepared. By reacting with sulfur-containing flue gas, zinc sulfate and EDTA-2Na are used to improve desulfurization and demagnesium Efficiency: Calcium hydroxide is added to precipitate to obtain magnesium hydroxide product.
It achieves efficient SO2 removal rate (up to 98%), improves the leaching rate of magnesium and phosphorus, reduces production costs, and the by-product magnesium hydroxide is economical, and the process is simple and easy to transform.
Smart Images

Figure CN118877844A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource utilization of phosphate ore, and specifically relates to a method for recovering magnesium and phosphorus resources in phosphate ore. Background Art
[0002] Phosphate rock is an important non-renewable and irreplaceable non-metallic mineral resource, which is widely used in agriculture, medicine, food, national defense, sugar production, new energy and other fields. Especially in agriculture, phosphate fertilizer, as one of the three important agricultural fertilizers, has a significant effect on increasing the yield of most crops. Many countries have included phosphate rock in the list of strategic mineral resources.
[0003] Extracting metal elements from phosphate ore is an economically valuable and important utilization method for the sustainable development of phosphate resources. Patent CN100392124C discloses the use of a composite demagnesizing agent containing sulfuric acid and at least one component selected from disodium ethylenediaminetetraacetate and nitric acid to demagnesify high-magnesium phosphate ore, so that magnesium in the phosphate ore is dissolved from the phosphate ore, and then a magnesium hydroxide product is obtained through precipitation reaction and solid-liquid separation. However, the patent only uses 98% sulfuric acid for demagnesizing, and the amount of disodium ethylenediaminetetraacetate added is too high, resulting in high costs. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention proposes a method for recovering magnesium and phosphorus resources in phosphate ore.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for recovering magnesium phosphorus resources in phosphate ore, comprising the following steps:
[0006] (1) grinding phosphate rock, zinc sulfate and disodium ethylenediaminetetraacetate to prepare phosphate slurry;
[0007] (2) using the phosphate slurry as an absorbent to enter a spray absorption tower to absorb the sulfur-containing flue gas in one turn and one absorption to perform desulfurization and demagnesium reactions to obtain a phosphate slurry after the reaction;
[0008] (3) Dehydrating the phosphate slurry after the reaction, and the dehydrated slag can be used as a raw material for the wet-process phosphoric acid process;
[0009] (4) adding calcium hydroxide to the liquid obtained by dehydration so that the pH of the supernatant is 8.0-8.5, centrifuging to obtain the supernatant, adding calcium hydroxide to the supernatant, and obtaining a precipitate as a magnesium hydroxide product.
[0010] As a preferred embodiment of the present invention, in the total mass of the phosphate rock, zinc sulfate and disodium EDTA, the mass percentage of zinc sulfate is 0.1-0.3%, and the mass percentage of disodium EDTA is 0.2-0.5%.
[0011] As a preferred embodiment of the present invention, in step (1), the solid-liquid mass ratio of the phosphate slurry is 25-40%.
[0012] As a preferred embodiment of the present invention, in the step (2), the absorption mode of the sulfur-containing flue gas by the phosphate slurry in the spray absorption tower is countercurrent absorption, and the spray layer of the spray absorption tower is provided with 3 layers, and the layer spacing is 1.5m.
[0013] As a preferred embodiment of the present invention, in step (2), in the spray absorption tower, the absorption temperature is 25-45°C; the gas flow rate is 0.5-3m / s; the gas includes sulfur-containing flue gas and oxygen, and the oxygen content is 5-20%; the liquid-gas ratio is 9-10L / m 3 .
[0014] As a preferred embodiment of the present invention, in step (2), the SO2 concentration in the sulfur-containing flue gas is 1000-5000 mg / m 3 , the flue gas volume is 10000-30000m 3 / h.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) This method adopts a countercurrent spray absorption tower. The phosphate ore is made into phosphate slurry in the slurry tank and passed into the top of the absorption tower for spraying. The tail gas of the "one-turn-one-absorption" process is passed into the bottom of the absorption tower and discharged from the top after absorption. The slurry after reaction is collected from the bottom to the dehydration device. The supernatant after dehydration enters the magnesium recovery workshop to extract magnesium. In this process, the removal rate of SO2 can reach more than 98%, and the highest can be close to 100%, which is lower than the SO2 specified in the flue gas emission standard GB18485-2014. x Emission concentration 80mg / Nm 3 .
[0017] (2) After adding zinc sulfate and EDTA-2Na to the phosphate slurry, the desulfurization efficiency is not affected, and the PO4 in the phosphate ore can be effectively improved. 3- The leaching rate of ore can reach about 110%, and the leaching rate of magnesium can reach more than 96%. Moreover, the liquid produced in this process can also be used as a raw material for magnesium production.
[0018] (3) The present invention organically combines the desulfurization of sulfur-containing flue gas in the "one-turn-one-absorption" process and the resource utilization of phosphate rock, which can not only achieve SO2 emission standards, but also make use of phosphate rock as a resource. The by-product Mg(OH)2 can also increase economic benefits. The process of the present invention is simple. On the basis of not changing or making little change to the existing wet flue gas purification equipment, it is easy to achieve process upgrade and transformation, thereby saving costs. The present invention uses phosphate rock for desulfurization and resource utilization, thereby realizing the resource utilization of sulfur dioxide and phosphate rock. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a flow chart of a method for recovering magnesium-phosphorus resources from phosphate ore. DETAILED DESCRIPTION
[0020] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0021] Example 1
[0022] like Figure 1 As shown, a method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0023] (1) 99.6% by weight of phosphate rock, 0.1% by weight of zinc sulfate, and 0.3% by weight of disodium ethylenediaminetetraacetate are ground to prepare a phosphate rock slurry with a solid-liquid mass ratio of 25%.
[0024] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated by one turn and one suction of sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 5%, and the SO2 concentration is 1000mg / m 3 , the smoke volume is 10000m 3 / h; the air velocity in the empty tower is 2m / s, and the liquid-gas ratio is: 9L / m 3 , the reaction temperature is 25℃, and the measured SO2 removal rate is 97.9%.
[0025] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the raw material for the wet phosphoric acid process. The leaching rate of magnesium can reach 96.8%, and PO4 3- The leaching rate is 95.6%.
[0026] (4) The dehydrated liquid is sent to a magnesium recovery workshop, calcium hydroxide is added to adjust the pH of the supernatant to 8.0-8.5, the supernatant and the solid are separated, and the solid is subsequently processed.
[0027] (5) adding an excess of calcium hydroxide to the supernatant, and then removing impurities from the precipitate, purifying it, dehydrating it, and drying it to obtain a solid having a magnesium hydroxide content of 96.4%.
[0028] Example 2
[0029] A method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0030] (1) 99.4% by weight of phosphate rock, 0.2% by weight of zinc sulfate, and 0.4% by weight of disodium ethylenediaminetetraacetate are ground to prepare a phosphate rock slurry with a solid-liquid mass ratio of 30%.
[0031] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated by one turn and one suction of sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 20%, and the SO2 concentration is 2000mg / m 3 , the flue gas volume is 15000m 3 / h; the air velocity in the tower is 3m / s, and the liquid-gas ratio is: 9.5L / m 3 , the reaction temperature is 35℃, and the measured SO2 removal rate is 98.4%.
[0032] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the raw material for the wet phosphoric acid process. The leaching rate of magnesium can reach 96.9%, and PO4 3- The leaching rate is 97.8%.
[0033] (4) The dehydrated liquid is sent to a magnesium recovery workshop, calcium hydroxide is added to adjust the pH of the supernatant to 8.0-8.5, the supernatant and the solid are separated, and the solid is subsequently processed.
[0034] (5) adding an excess of calcium hydroxide to the supernatant, and then removing impurities from the precipitate, purifying it, dehydrating it, and drying it to obtain a solid having a magnesium hydroxide content of 95.8%.
[0035] Example 3
[0036] A method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0037] (1) 99.2% by weight of phosphate rock, 0.3% by weight of zinc sulfate, and 0.5% by weight of disodium ethylenediaminetetraacetate are ground to prepare a phosphate rock slurry with a solid-liquid mass ratio of 30%.
[0038] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated by one turn and one suction of sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 15%, and the SO2 concentration is 5000mg / m 3 , the flue gas volume is 30000m 3 / h; the air velocity in the tower is 0.5m / s, and the liquid-gas ratio is: 10L / m 3 , the reaction temperature is 45℃, and the measured SO2 removal rate is 98.7%.
[0039] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the raw material for the wet phosphoric acid process. The leaching rate of magnesium can reach 98.4%, PO4 3- The leaching rate is 97.3%.
[0040] (4) The dehydrated liquid is sent to a magnesium recovery workshop, calcium hydroxide is added to adjust the pH of the supernatant to 8.0-8.5, the supernatant and the solid are separated, and the solid is subsequently processed.
[0041] (5) adding an excess of calcium hydroxide to the supernatant, and then removing impurities from the precipitate, purifying it, dehydrating it, and drying it to obtain a solid having a magnesium hydroxide content of 94.3%.
[0042] Comparative Example 1
[0043] A method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0044] (1) Grinding phosphate rock with a mass percentage of 99.7% and disodium ethylenediaminetetraacetate with a mass percentage of 0.3% to prepare phosphate slurry with a solid-liquid mass ratio of 25%.
[0045] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated in a one-turn-one-absorption sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 5%, and the SO2 concentration is 1500mg / m 3 , the smoke volume is 10000m 3 / h; the air velocity in the empty tower is 2m / s, and the liquid-gas ratio is: 9L / m 3 , the reaction temperature is 25℃, and the measured SO2 removal rate is 98.7%.
[0046] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the raw material for the wet phosphoric acid process. The leaching rate of magnesium can reach 87.8%, and PO4 3- The leaching rate is 84.9%.
[0047] (4) The dehydrated liquid is sent to a magnesium recovery workshop, calcium hydroxide is added to adjust the pH of the supernatant to 8.0-8.5, the supernatant and the solid are separated, and the solid is subsequently processed.
[0048] (5) adding an excess of calcium hydroxide to the supernatant, and then removing impurities from the precipitate, purifying it, dehydrating it, and drying it to obtain a solid having a magnesium hydroxide content of 89.6%.
[0049] Comparative Example 2
[0050] A method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0051] (1) 99.7% by weight phosphate rock and 0.3% by weight zinc sulfate are ground to prepare a phosphate rock slurry with a solid-liquid mass ratio of 25%.
[0052] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated in a one-turn-one-absorption sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 5%, and the SO2 concentration is 1500mg / m 3 , the smoke volume is 10000m 3 / h; the air velocity in the empty tower is 2m / s, and the liquid-gas ratio is: 9L / m 3 , the reaction temperature is 25℃, and the measured SO2 removal rate is 99.4%.
[0053] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the raw material for the wet phosphoric acid process. The leaching rate of magnesium can reach 91.4%, PO4 3- The leaching rate is 87.4%.
[0054] (4) The dehydrated liquid is sent to a magnesium recovery workshop, calcium hydroxide is added to adjust the pH of the supernatant to 8.0-8.5, the supernatant and the solid are separated, and the solid is subsequently processed.
[0055] (5) adding an excess of calcium hydroxide to the supernatant, and then removing impurities from the precipitate, purifying it, dehydrating it, and drying it to obtain a solid having a magnesium hydroxide content of 91.6%.
[0056] Comparative Example 3
[0057] A method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0058] (1) grinding phosphate rock with a mass percentage of phosphate rock to prepare a phosphate rock slurry with a solid-liquid mass ratio of 25%.
[0059] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated in a one-turn-one-absorption sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 5%, and the SO2 concentration is 1500mg / m 3 , the smoke volume is 10000m 3 / h; the air velocity in the empty tower is 2m / s, and the liquid-gas ratio is: 9L / m 3 , the reaction temperature is 25℃, and the measured SO2 removal rate is 99.2%.
[0060] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the wet phosphoric acid process principle. The leaching rate of magnesium can reach 75.3%, PO4 3- The leaching rate is 73.9%.
[0061] (4) The dehydrated liquid is sent to a magnesium recovery workshop, calcium hydroxide is added to adjust the pH of the supernatant to 8.0-8.5, the supernatant and the solid are separated, and the solid is subsequently processed.
[0062] (5) adding an excess of calcium hydroxide to the supernatant, and then removing impurities from the precipitate, purifying it, dehydrating it, and drying it to obtain a solid having a magnesium hydroxide content of 84.5%.
[0063] It can be seen from the comparison between Example 1 and Example 1-3 that zinc sulfate and disodium ethylenediaminetetraacetic acid work synergistically to improve the leaching of magnesium and phosphorus and the content of magnesium hydroxide in the solid. Zinc sulfate can separate calcium fluorophosphate (Ca5(PO4)3F) and calcium magnesium carbonate (CaMg(CO3)2) in phosphate ore, but sulfate radicals generated in sulfur dioxide react with the above two substances to produce calcium sulfate (CaSO4·2H2O) attached to the particle surface, thereby inhibiting the leaching of magnesium and phosphorus. Adding disodium ethylenediaminetetraacetic acid can occupy the active site of calcium sulfate generation, thereby strengthening the leaching of magnesium and phosphorus.
[0064] Comparative Example 4
[0065] A method for recovering magnesium-phosphorus resources in phosphate ore comprises the following steps:
[0066] (1) 99.6% by weight of phosphate rock, 0.1% by weight of zinc sulfate, and 0.3% by weight of disodium ethylenediaminetetraacetate are ground to prepare a phosphate rock slurry with a solid-liquid mass ratio of 25%.
[0067] (2) Phosphate slurry is used as absorbent and sent to the countercurrent spray absorption tower through the circulating pump pipeline for desulfurization and demagnesium reaction. The spray layer is set up with 3 layers, and the layer spacing is 1.5m. The flue gas is treated by one turn and one suction of sulfur-containing flue gas. The oxygen concentration in the sulfur-containing flue gas is 5%, and the SO2 concentration is 1000mg / m 3 , the smoke volume is 10000m 3 / h; the air velocity in the empty tower is 2m / s, and the liquid-gas ratio is: 9L / m 3 , the reaction temperature is 25℃, and the measured SO2 removal rate is 97.9%.
[0068] (3) Dehydrate the phosphate slurry after the reaction, and use the dehydrated slag as the raw material for the wet phosphoric acid process. The leaching rate of magnesium can reach 95.5%, PO4 3- The leaching rate is 96.1%.
[0069] (4) The dehydrated liquid is sent to a magnesium recovery workshop, excess calcium hydroxide is added, and then the precipitate is purified, dehydrated and dried to obtain a solid with a magnesium hydroxide content of 85.0%.
[0070] Compared with Example 1, Comparative Example 4, the present invention uses a two-stage neutralization method, which can overcome the situation that the precipitate obtained by one-stage neutralization precipitation contains a large amount of impurities, resulting in a low magnesium hydroxide content.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for recovering magnesium and phosphorus resources from phosphate ore, characterized in that: The steps include: (1) grinding phosphate rock, zinc sulfate and disodium ethylenediaminetetraacetate to prepare phosphate slurry; (2) using the phosphate slurry as an absorbent to enter a spray absorption tower to absorb the sulfur-containing flue gas in one turn and one absorption to perform desulfurization and demagnesium reactions to obtain a phosphate slurry after the reaction; (3) dehydrating the phosphate slurry after the reaction to obtain slag after dehydration; (4) adding calcium hydroxide to the liquid obtained by dehydration so that the pH of the supernatant is 8.0-8.5, centrifuging to obtain the supernatant, adding calcium hydroxide to the supernatant, and obtaining a precipitate as a magnesium hydroxide product.
2. The method for recovering magnesium and phosphorus resources from phosphate ore according to claim 1, characterized in that: In the total mass of the phosphate rock, zinc sulfate and disodium ethylenediaminetetraacetate, the mass percentage of zinc sulfate is 0.1-0.3%, and the mass percentage of disodium ethylenediaminetetraacetate is 0.2-0.5%.
3. The method for recovering magnesium-phosphorus resources in phosphate ore according to claim 1, characterized in that: In the step (1), the solid-to-liquid ratio of the phosphate slurry is 25-40%.
4. The method for recovering magnesium-phosphorus resources in phosphate ore according to claim 1, characterized in that: In the step (2), the absorption mode of the sulfur-containing flue gas by the phosphate slurry in the spray absorption tower is countercurrent absorption, and the spray layer of the spray absorption tower is provided with 3 layers, and the layer spacing is 1.5m.
5. The method for recovering magnesium and phosphorus resources from phosphate ore according to claim 1, characterized in that: In the step (2), in the spray absorption tower, the absorption temperature is 25-45°C; the gas flow rate is 0.5-3m / s; the gas includes sulfur-containing flue gas and oxygen, and the oxygen content is 5-20%; the liquid-gas ratio is 9-10L / m 3 .
6. The method for recovering magnesium and phosphorus resources from phosphate ore according to claim 1, characterized in that: In step (2), the SO2 concentration in the sulfur-containing flue gas is 1000-5000 mg / m 3 , the flue gas volume is 10000-30000m 3 / h.
Citation Information
Patent Citations
Method for recycling magnesium from middle-low grade high-magnesium phosphate rock
CN102115819A
Method for removing magnesium from ultralow-quality phosphate rock and producing magnesium hydroxide
CN103073034A
Method for removing SO2 and NOX from flue gas of coal-fired boiler by virtue of phosphoric ore pulp and phosphorus sludge
CN105536493A
Flue gas desulfurization method and system based on ammonia-magnesium combined reinforced phosphoric ore pulp method
CN111437712A
Method of retrieving magnesium from high magnesium phosphorus ore
CN1924046A