Quartz sand pellet as well as preparation method and application thereof
The pellets made from quartz sand of different purity and particle sizes are solved by combining the melt roasting technology, and the problems of environmental impact and low resource utilization efficiency in the existing technology are solved, and the production and cost reduction of high-purity industrial silicon are achieved. .
Patent Information
- Application Number
- CN202411018662.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing industrial silicon smelting technology, the mining and processing of silica raw materials have a great impact on the environment, and it is difficult to effectively utilize low-grade quartz sand, resulting in low resource utilization efficiency.
The pellets are made of quartz sand of different purity and particle sizes, and through melt roasting technology, high-hardness and dense quartz sand pellets are formed, which are used to replace the combination of silica and carbonaceous reducing agent for smelting to produce high-quality industrial silicon.
It realizes efficient utilization of low-grade quartz sand, produces high-purity industrial silicon, reduces production costs, meets the furnace hardness requirements of industrial silicon smelting, and improves resource utilization efficiency.
Smart Images

Figure CN118877894A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of efficient and clean utilization of resources, and specifically relates to a quartz sand pellet, a preparation method and application thereof. Background Art
[0002] Most of the existing industrial silicon smelting technologies are to mix silica and carbonaceous reducing agents in one or more arbitrary proportions for smelting, and their products are widely used in the refractory and concrete industries.
[0003] As a new type of material, quartz sand pellets can replace traditional silica for smelting due to their high purity and excellent high temperature resistance. In addition, from the perspective of environmental protection and resource utilization, the use of quartz sand pellets instead of silica also has certain advantages. Since quartz sand pellets can be prepared in a more environmentally friendly way and low-grade quartz sand can be recycled, compared with the traditional silica mining and processing process, it has less impact on the environment.
[0004] Therefore, it is of great significance to develop a method for producing high-quality industrial silicon by using mixed quartz sand pellets instead of silica. This is not only in line with the current trend of global environmental protection, but also helps to improve the efficiency of resource utilization. So far, there has been no report on the process of melting and roasting quartz sand of different purities before silicon smelting, and then adding a reducing agent for smelting. Summary of the invention
[0005] The present invention aims at the problem of smelting silica raw materials for industrial silicon in the prior art, and provides a method for producing high-quality industrial silicon by using mixed quartz sand pellets instead of silica. The present invention uses quartz sands of different purities and different particle sizes as raw materials, improves the strength of the pellets by the hardness of fused quartz itself, and bakes quartz sands of different particle sizes to make the pellets form a more compact structure, while improving the hardness of the pellets. The pellets of the present invention can ensure that the silica furnace charge reaches the hardness of entering the furnace during use, can replace silica and combine with a reducing agent to produce high-quality industrial silicon, and can be fully used for the smelting and production of industrial silicon.
[0006] The present invention is based on previous research (such as patent 2023108529864) to further reduce costs and efficiently utilize resources. It is found that under the same process conditions, the product quality of the present invention is significantly improved compared with the product of CN116873931A, and the present invention also realizes the preparation of high-purity silicon using low-grade quartz sand for the first time.
[0007] The quartz sand pellets of the present invention are prepared by using quartz sand of different purities and particle sizes as raw materials, adding water and a binder, stirring the mixture evenly, putting it into a mold and pressing it into a pellet, and calcining it at a temperature greater than or equal to 1750° C., preferably 1780-1820° C., to obtain calcined quartz sand pellets;
[0008] Quartz sand of different purities includes high-purity quartz sand, ordinary quartz sand and low-grade quartz sand; the particle size of high-purity quartz sand is larger than that of ordinary quartz sand, and the particle size of ordinary quartz sand is larger than that of low-grade quartz sand; the mass of high-purity quartz sand is greater than that of ordinary quartz sand, and the mass of ordinary quartz sand is greater than that of low-grade quartz sand; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40-50:20-30:10-20.
[0009] The invention discloses a quartz sand pellet, wherein the particle size of the high-purity quartz sand is 106-180 microns; in the high-purity quartz sand, SiO2≥99.5wt%; preferably, in the high-purity quartz sand, in terms of mass percentage, SiO2≥99.5%, Fe2O3≤0.05%, Al2O3≤0.05%, and CaO≤0.05%;
[0010] The particle size of ordinary quartz sand is 83 to 106 microns; 99.5wt%>SiO2≥95wt% in ordinary quartz sand; preferably, in ordinary quartz sand, by mass percentage, SiO2≥95%, Fe2O3≤0.10%, Al2O3≤0.10%, CaO≤0.10%, and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0011] The particle size of the low-grade quartz sand is less than 83 microns; in the low-grade quartz, 95wt%>SiO2≥90wt%; preferably, in the low-grade quartz, by mass percentage, SiO2≥90%, Fe2O3≤0.20%, Al2O3≤0.20%, CaO≤0.20%, and the content of silicon dioxide in the low-grade quartz is less than that in ordinary quartz sand.
[0012] The present invention provides a method for preparing quartz sand pellets, the method comprising the following steps:
[0013] Step 1, firstly crushing high-purity quartz sand, ordinary quartz sand and low-grade quartz sand into particles of required particle size; wherein the particle size of high-purity quartz sand is 106-180 microns, the particle size of ordinary quartz sand is 83-105 microns, and the particle size of low-grade quartz sand is less than 83 microns;
[0014] Step 2, first add 5wt% to 6wt% of water and 1.4 to 1.6wt%, preferably 1.5wt% of a binder to high-purity quartz sand, and stir evenly to obtain a mixture A;
[0015] Step 3, adding ordinary quartz sand to the mixture A of step 2, and then adding 5wt% to 6wt.% of water relative to the mass of the ordinary quartz sand, and 1.4 to 1.6wt.%, preferably 1.5wt.% of a binder; stirring evenly to obtain a mixture B;
[0016] Step 4, adding low-grade quartz sand to the mixture B of step 3, and then adding 5wt% to 6wt.% of water relative to the mass of the low-grade quartz sand itself, and 1.4 to 1.6wt.%, preferably 1.5wt.% of a binder; stirring evenly to obtain a mixture C;
[0017] Step 5, placing the mixed material C stirred evenly in step 4 into a mold and pressing it into a mass, and placing it in a drying oven at 80-120°C, preferably at 100°C, and drying it for 3-5 hours, preferably 200-260 minutes; in an air-tight condition, low-temperature roasting the formed mass at a temperature greater than or equal to 1750°C, preferably at 1780-1820°C, and keeping it warm for 4-6 hours, and cooling it to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0018] In the present invention, if the pellets are not dried, they will enter the high-temperature roasting zone (1800°C) with a large amount of water, and the water in the pellets will evaporate violently, causing the green pellets to crack or even explode.
[0019] Because too fine a particle size will make it difficult to form a pellet, and will make the surface of the pellet smooth, which is not conducive to the weight gain of the pellet; too coarse a particle size will make the structure of the pellet loose and easy to break; and the overall purity of the mixed pellet must be guaranteed; so the present invention first mixes high-purity quartz sand with a large particle size with an appropriate amount of binder and water, and then mixes ordinary quartz sand with a slightly smaller particle size + binder + water again, and finally mixes low-grade quartz sand with a smaller particle size + binder + water again. Doing so can prioritize the formation of the pellet internally and also ensure the weight of the pellet; in order to prevent the pellet structure from being loose, two layers of small-particle quartz sand are mixed externally to ensure that the pellet structure is compact and not easy to fall apart. If this is not done, the pellet structure will be unstable, and the smooth formation of the pellet cannot be guaranteed.
[0020] The invention discloses a method for preparing quartz sand pellets. When the particle size of high-purity quartz sand is 150-180 microns, the particle size of common quartz sand is 106-125 microns, and the particle size of low-grade quartz sand is 83-90 microns, the mass ratio of high-purity quartz sand, common quartz sand and low-grade quartz sand is 50:20:10.
[0021] The invention discloses a method for preparing quartz sand pellets. When the particle size of high-purity quartz sand is greater than or equal to 125 microns and less than 150 microns, the particle size of common quartz sand is greater than or equal to 96 microns and less than 106 microns, and the particle size of low-grade quartz sand is 75-80 microns, the mass ratio of high-purity quartz sand, common quartz sand and low-grade quartz sand is 45:25:15.
[0022] The invention discloses a method for preparing quartz sand pellets. The particle size of high-purity quartz sand is greater than or equal to 109 microns and less than 125 microns; the particle size of common quartz sand is greater than or equal to 80 microns and less than 96 microns; the particle size of low-grade quartz sand is 50 to 75 microns;
[0023] The mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40:30:20.
[0024] The invention discloses a method for preparing quartz sand pellets. The binder in step 2, step 3 and step 4 is an organic-inorganic composite binder, wherein the inorganic binder accounts for 9.5-21 wt.% of the composite binder, and the organic binder accounts for 79-90.5 wt.%; the inorganic binder is selected from water glass; and the organic binder is selected from microcrystalline cellulose.
[0025] Preferably, in a method for preparing quartz sand pellets of the present invention, when the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40:30:20,
[0026] or
[0027] When the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10,
[0028] The binder in step 2, step 3 and step 4 is an organic-inorganic composite binder, in which the inorganic binder accounts for 19.5-20.5wt% and the organic binder accounts for 79.5-80.5wt%; the inorganic binder is selected from water glass; and the organic binder is selected from microcrystalline cellulose.
[0029] Preferably, in a method for preparing quartz sand pellets of the present invention, when the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 45:25:15,
[0030] The binder in step 2, step 3 and step 4 is an organic-inorganic composite binder, in which the inorganic binder accounts for 10-10.5wt% and the organic binder accounts for 90.5-90wt%; the inorganic binder is selected from water glass; and the organic binder is selected from microcrystalline cellulose.
[0031] The invention discloses a method for preparing quartz sand pellets. The diameter of the obtained quartz sand pellets for industrial silicon is 50-60 mm, including 53-58 mm.
[0032] The invention discloses an application of quartz sand pellets, comprising mixing quartz sand pellets and a carbonaceous reducing agent in a mass ratio of quartz sand pellets: carbonaceous reducing agent = 0.95-1.05:0.95-1.1, preferably 0.95-1:1-1.05, uniformly, and then adding the mixture into a submerged arc furnace for smelting at a temperature of 2000-2300 degrees Celsius to obtain industrial silicon.
[0033] In the present invention, the silicon yield refers to the ratio of 1 ton to the mass (t) of quartz sand pellets consumed in producing one ton of silicon. The silicon yield = 1 ton / unit consumption of quartz sand pellets * 100%.
[0034] By adopting the process of the present invention, after adding a reducing agent to the obtained pellets and smelting, the Mohs hardness is tested to reach 7, which meets the requirements of industrial silicon smelting furnace, the silicon output rate is 38.3% to 42.6%, and the purity of the obtained industrial silicon is greater than or equal to 99.2%.
[0035] After optimization, the silicon yield was 42.6% and the silicon purity was 99.4wt%.
[0036] The present invention realizes for the first time the use of low-purity (such as silicon dioxide grade of 90-95%) silica as raw material, and through the improvement of pelletizing technology, it can be used to prepare high-quality industrial silicon (silicon purity greater than or equal to 99.2%).
[0037] The beneficial effects of the present invention are:
[0038] 1. The present invention uses quartz sand of different purities and different particle sizes as raw materials, uses the hardness of fused quartz itself to improve the strength of the pellets, and bakes quartz sand of different particle sizes to make the pellets form a denser structure, while improving the hardness of the pellets (its Mohs hardness is greater than or equal to level 7).
[0039] 2. The pellets can ensure that the mixed charge reaches the hardness of entering the furnace during use. They can replace silica and combine with reducing agents to produce high-quality industrial silicon, which can be fully used for the smelting and production of industrial silicon.
[0040] 3. After being calcined at 1800° C., the mixed quartz sand pellets prepared by the present invention have a Mohs hardness of 7, which meets the requirements for entering the furnace for industrial silicon smelting and is fully applicable to the smelting and production of industrial silicon.
[0041] 4. The mixed quartz sand pellets prepared by the present invention are used in industrial silicon smelting, can replace silica and combine with a reducing agent to produce high-quality industrial silicon, and the obtained industrial silicon with Si≥99.2wt% can be obtained after optimization. Industrial silicon with Si≥99.4wt% can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The present invention is a flow chart for the production of mixed quartz sand pellets. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0044] Example 1
[0045] A method for producing high-quality industrial silicon from quartz sand pellets, wherein the obtained pellets are smelted and tested to have a Mohs hardness greater than or equal to 7, meeting the requirements for industrial silicon smelting into a furnace;
[0046] The mixed quartz sand pellets are prepared by the following steps:
[0047] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; wherein the particle size of high-purity quartz sand is greater than or equal to 109 microns and less than 125 microns; the particle size of ordinary quartz sand is greater than or equal to 80 microns and less than 96 microns; the particle size of low-grade quartz sand is 50-75 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40:30:20;
[0048] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0049] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to the mass of ordinary quartz sand and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0050] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to the mass of the low-grade quartz sand and 1.5wt.% of a binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0051] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0052] The raw materials used:
[0053] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0054] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0055] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%; and the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0056] 98kg of the above mixed quartz sand pellets were evenly mixed with 102kg of carbonaceous reducing agent, and added into a submerged arc furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 39.5%, and the composition of the industrial silicon product was Si>99.25wt.%, Fe≤0.19wt.%, Al≤0.09Wt.%, and Ca≤0.05Wt.%.
[0057] Example 2
[0058] A method for producing high-quality industrial silicon from quartz sand pellets, wherein the obtained pellets are smelted and tested to have a Mohs hardness greater than or equal to 7, meeting the requirements for industrial silicon smelting into a furnace;
[0059] The mixed quartz sand pellets are prepared by the following steps:
[0060] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; wherein the particle size of high-purity quartz sand is greater than or equal to 109 microns and less than 125 microns; the particle size of ordinary quartz sand is greater than or equal to 80 microns and less than 96 microns; the particle size of low-grade quartz sand is 50-75 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40:30:20;
[0061] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt% and the organic binder accounts for 90wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0062] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to the mass of ordinary quartz sand and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt.%, and the organic binder accounts for 90wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0063] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to the mass of the low-grade quartz sand and 1.5wt.% of a binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt.%, and the organic binder accounts for 90wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0064] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0065] The raw materials used:
[0066] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0067] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0068] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%; and the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0069] 100kg of the above mixed quartz sand pellets were evenly mixed with 100kg of carbonaceous reducing agent, and added into a submerged arc furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 38.3%, and the composition of the industrial silicon product was Si>99.2wt.%, Fe≤0.19wt.%, Al≤0.09Wt.%, and Ca≤0.05Wt.%.
[0070] Example 3
[0071] A method for producing high-quality industrial silicon from quartz sand pellets. After smelting, the obtained pellets have a Mohs hardness of 7, which meets the requirements for smelting industrial silicon into a furnace.
[0072] The mixed quartz sand pellets are prepared by the following steps:
[0073] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; the particle size of high-purity quartz sand is greater than or equal to 125 microns and less than 150 microns; the particle size of ordinary quartz sand is greater than or equal to 90 microns and less than 106 microns; the particle size of low-grade quartz sand is 75-80 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 45:25:15;
[0074] Step 2: first add 5wt% water relative to its own mass and 1.5wt% binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0075] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 5wt.% water relative to the mass of ordinary quartz sand and 1.5wt.% binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0076] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 5wt.% of water relative to the mass of the low-grade quartz sand and 1.5wt.% of a binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0077] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0078] The raw materials used:
[0079] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0080] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0081] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%; and the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0082] 100kg of the above mixed quartz sand pellets were evenly mixed with 100kg of carbonaceous reducing agent, and added into a submerged arc furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 40.8%, and the composition of the industrial silicon product was Si>99.3wt.%, Fe≤0.19wt.%, Al≤0.09Wt.%, and Ca≤0.05Wt.%.
[0083] Example 4
[0084] A method for producing high-quality industrial silicon from quartz sand pellets. After smelting, the obtained pellets have a Mohs hardness of 7, which meets the requirements for smelting industrial silicon into a furnace.
[0085] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0086] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; the particle size of high-purity quartz sand is greater than or equal to 125 microns and less than 150 microns; the particle size of ordinary quartz sand is greater than or equal to 96 microns and less than 106 microns; the particle size of low-grade quartz sand is 75-80 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 45:25:15;
[0087] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt% and the organic binder accounts for 90wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0088] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt.%, and the organic binder accounts for 90wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0089] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt.%, and the organic binder accounts for 90wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0090] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0091] The raw materials used:
[0092] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0093] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0094] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0095] 98kg of the above mixed quartz sand pellets were evenly mixed with 102kg of carbonaceous reducing agent, and added into a submerged arc furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 41.7%, and the composition of the industrial silicon product was Si>99.35wt.%, Fe≤0.19wt.%, Al≤0.09Wt.%, and Ca≤0.05Wt.%.
[0096] Example 5
[0097] A method for producing high-quality industrial silicon from quartz sand pellets. After smelting, the obtained pellets have a Mohs hardness of 7, which meets the requirements for smelting industrial silicon into a furnace.
[0098] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0099] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; the particle size of high-purity quartz sand is greater than or equal to 150 microns and less than 180 microns; the particle size of ordinary quartz sand is greater than or equal to 106 microns and less than 125 microns; the particle size of low-grade quartz sand is 80-96 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10;
[0100] Step 2: first add 5wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0101] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 5wt.% water relative to the mass of ordinary quartz sand and 1.5wt.% binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0102] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 5wt.% of water relative to the mass of the low-grade quartz sand and 1.5wt.% of a binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0103] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0104] The raw materials used:
[0105] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0106] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0107] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0108] 100kg of the above mixed quartz sand pellets were evenly mixed with 100kg of carbonaceous reducing agent, and added into a submerged arc furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 42.2%, and the composition of the industrial silicon product was Si>99.38wt.%, Fe≤0.19wt.%, Al≤0.09Wt.%, and Ca≤0.05Wt.%.
[0109] Example 6
[0110] A method for producing high-quality industrial silicon from quartz sand pellets. After smelting, the obtained pellets have a Mohs hardness of 7, which meets the requirements for smelting industrial silicon into a furnace.
[0111] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0112] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; the particle size of high-purity quartz sand is greater than or equal to 150 microns and less than 180 microns; the particle size of ordinary quartz sand is greater than or equal to 106 microns and less than 125 microns; the particle size of low-grade quartz sand is 80-96 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10;
[0113] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt% and the organic binder accounts for 90wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0114] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt.%, and the organic binder accounts for 90wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0115] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 10wt.%, and the organic binder accounts for 90wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0116] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0117] The raw materials used:
[0118] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0119] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0120] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0121] 98kg of the above mixed quartz sand pellets were evenly mixed with 102kg of carbonaceous reducing agent, and added into a submerged arc furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 42.6%, and the composition of the industrial silicon product was Si>99.4wt.%, Fe≤0.19wt.%, Al≤0.09Wt.%, and Ca≤0.05Wt.%.
[0122] Comparative Example 1
[0123] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0124] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; the particle size of high-purity quartz sand is greater than or equal to 106 microns and less than 125 microns; the particle size of ordinary quartz sand is greater than or equal to 80 microns and less than 96 microns; the particle size of low-grade quartz sand is 50-75 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10;
[0125] Step 2: Mix high-purity quartz sand, ordinary quartz sand, and low-grade quartz sand all at once in no particular order, and add 6wt.% of water and 1.5wt.% of a binder relative to the total mass of the three quartz sand mixture at once, and stir until the mixture is completely mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0126] Step 3, the mixed material stirred evenly in step 2 is placed in a mold and pressed into agglomerate particles with a diameter of 55 mm, and then placed in a drying oven at 100° C. for 4 hours. The formed agglomerates are placed in an air-tight state at a temperature of 1800° C. for high temperature calcination, kept warm for 4 hours, and cooled to room temperature with the furnace to obtain quartz sand pellets, but the hardness of the obtained quartz sand pellets is less than level 7.
[0127] The raw materials used:
[0128] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0129] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0130] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0131] Since there was no sequence in the mixing process, the pellets were not uniform as a whole, and they were heated unevenly during the drying process. The lumps could not be formed due to cracking, and the final product could not reach the required hardness before entering the furnace. Therefore, the mixing failed and it was impossible to make pellets by mixing the three types of quartz sand at one time.
[0132] Comparative Example 2
[0133] A method for producing high-quality industrial silicon from quartz sand pellets. After smelting, the obtained pellets have a Mohs hardness of 7, which meets the requirements for smelting industrial silicon into a furnace.
[0134] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0135] Step 1, firstly crush high-purity quartz sand and low-grade quartz sand, and screen them into particles of required particle size; wherein the particle size of high-purity quartz sand is greater than or equal to 125 microns and less than 150 microns, and the particle size of low-grade quartz sand is greater than or equal to 80 microns and less than 96 microns. The mass ratio of high-purity quartz sand to low-grade quartz sand is 55:25;
[0136] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0137] Step 3, adding low-grade quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0138] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0139] The raw materials used:
[0140] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0141] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in high-purity quartz sand;
[0142] 98kg of the above mixed quartz sand pellets were mixed evenly with 102kg of carbonaceous reducing agent and added into the ore-fired furnace for smelting (the smelting temperature was 2300 degrees Celsius). The furnace smelting was stable, the silicon yield was 39.15%, and the composition of the industrial silicon product was S i >98.25Wt.%, Fe≤0.21wt.%, Al≤0.11Wt.%, Ca≤0.07Wt.%.
[0143] Since the purity of the final product silicon obtained by this scheme did not reach the standard of 98.7Wt.% for industrial silicon products, and the high proportion of high-purity quartz sand used resulted in excessively high costs, this scheme failed, and it was not possible to use only high-purity quartz sand and low-grade quartz sand to mix and produce quartz sand pellets that met the needs of industrial silicon.
[0144] Comparative Example 3
[0145] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0146] Step 1: First, high-purity quartz sand, ordinary quartz sand, and low-grade quartz sand are crushed and screened into particles of the required particle size. The three types of quartz sand have the same particle size, which is 96 to 106 microns.
[0147] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0148] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0149] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0150] Step 5, put the mixture stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature calcination, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
[0151] The raw materials used:
[0152] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0153] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0154] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0155] Since the three types of quartz sand have the same particle size, although the mixing and tableting can proceed normally, the heat distribution of the agglomerates is uneven during the drying process, which affects the consolidation effect of the pellets and the compressive strength of the green balls, resulting in the final product failing to reach the required furnace hardness (Mohs hardness less than 7). Therefore, the mixing failed and it is impossible to make pellets by mixing three types of quartz sand with the same particle size but different purity.
[0156] Comparative Example 4
[0157] A method for producing high-quality industrial silicon from quartz sand pellets. After smelting, the obtained pellets have a Mohs hardness of 7, which meets the requirements for smelting industrial silicon into a furnace.
[0158] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0159] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; wherein the particle size of high-purity quartz sand is 50-75 microns, the particle size of ordinary quartz sand is 80-96 microns, and the particle size of low-grade quartz sand is 106-125 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10;
[0160] Step 2: first add 6wt% of water relative to its own mass and 1.5wt% of binder to high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0161] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0162] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to its own mass and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0163] Step 5, put the mixed material stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for drying for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature baking, keep warm for 4 hours, and cool to room temperature with the furnace to obtain quartz sand pellets.
[0164] The raw materials used:
[0165] The chemical composition of high-purity quartz sand is SiO2 ≥ 99.5%, Fe2O3 ≤ 0.05%, Al2O3 ≤ 0.05%, CaO ≤ 0.05%;
[0166] The chemical composition of ordinary quartz sand is SiO2 ≥ 95%, Fe2O3 ≤ 0.10%, Al2O3 ≤ 0.10%, CaO ≤ 0.10%; and the content of silicon dioxide in ordinary quartz sand is less than that in high-purity quartz sand;
[0167] The chemical composition of low-grade quartz sand is SiO2 ≥ 90%, Fe2O3 ≤ 0.20%, Al2O3 ≤ 0.20%, CaO ≤ 0.20%. And the content of silicon dioxide in low-grade quartz sand is less than that in ordinary quartz sand;
[0168] Since the particle size of the pellets gradually increases from the inside to the outside during mixing, the stability of the green balls during calcination cannot be guaranteed. Although the mixing and tableting can be carried out normally, during the drying process, due to the thick outer layer of the pellets, the heat cannot enter the center of the pellets, the heat distribution of the agglomerates is uneven, the consolidation effect of the pellets is poor, and the compressive strength of the green balls cannot meet the standard, resulting in the final product failing to reach the required furnace hardness (Mohs hardness less than 7). Therefore, the mixing failed and the pellets could not be made by mixing fine-grained high-purity quartz sand, medium-grained ordinary quartz sand, and large-grained low-grade quartz sand.
[0169] Comparative Example 5
[0170] The mixed quartz sand pellets are prepared by the following steps, comprising the steps of:
[0171] Step 1, firstly crush high-purity quartz sand, ordinary quartz sand and low-grade quartz sand, and screen them into particles of required particle size; wherein the particle size of high-purity quartz sand is 50-75 microns, the particle size of ordinary quartz sand is 106-125 microns, and the particle size of low-grade quartz sand is 80-96 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10;
[0172] Step 2: first add 6wt% of water relative to the mass of the high-purity quartz sand and 1.5wt% of a binder to the high-purity quartz sand and stir until the mixture is evenly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt% and the organic binder accounts for 80wt%. The inorganic binder is water glass and the organic binder is microcrystalline cellulose.
[0173] Step 3, adding ordinary quartz sand to the mixture of step 2, and then adding 6wt.% of water relative to the mass of ordinary quartz sand and 1.5wt.% of binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0174] Step 4, adding low-grade quartz sand to the mixture of step 3, and then adding 6wt.% of water relative to the mass of the low-grade quartz sand and 1.5wt.% of a binder and stirring until the mixture is uniformly mixed, wherein the binder is an organic-inorganic composite binder, in which the inorganic binder accounts for 20wt.%, and the organic binder accounts for 80wt.%, the inorganic binder is water glass, and the organic binder is microcrystalline cellulose.
[0175] Step 5, put the mixed material stirred evenly in step 4 into a mold and press it into agglomerate particles with a diameter of 55 mm, and put it into a 100°C drying oven for drying for 4 hours; place the formed agglomerates at a temperature of 1800°C in an air-tight manner for high temperature baking, keep warm for 4 hours, and cool them to room temperature to obtain quartz sand pellets (Mohs hardness less than level 7).
[0176] Since the particle size of the pellets increases first and then decreases from the inside to the outside during mixing, the internal structure of the pellets is uneven. Although mixing and tableting can proceed normally, during the drying process, the heat from the outer layer of the pellets can be conducted to the middle layer. However, the thickness of the middle layer is large, resulting in the heat being unable to enter the inner layer, i.e., the center of the pellets. The heat distribution of the agglomerates is uneven, the consolidation effect of the pellets is poor, and the compressive strength of the raw balls cannot meet the standard, resulting in the final product being unable to achieve the required hardness before entering the furnace. Therefore, this mixing also failed, and it was impossible to make pellets by mixing fine-grained high-purity quartz sand, large-grained ordinary quartz sand, and medium-grained low-grade quartz sand.
[0177] The specific embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A quartz sand pellet, which uses quartz sand of different purity and particle size as raw material, adds water and a binder, stirs the mixture evenly, puts it into a mold and presses it into a pellet, and calcines it at a temperature greater than 1750°C to obtain the calcined quartz sand pellet; characterized by: Quartz sand of different purities includes high-purity quartz sand, ordinary quartz sand and low-grade quartz sand; the particle size of high-purity quartz sand is larger than that of ordinary quartz sand, and the particle size of ordinary quartz sand is larger than that of low-grade quartz sand; the mass of high-purity quartz sand is greater than that of ordinary quartz sand, and the mass of ordinary quartz sand is greater than that of low-grade quartz sand; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40-50:20-30:10-20.
2. The quartz sand pellet according to claim 1, characterized in that: The particle size of high-purity quartz sand is 106-180 microns; in high-purity quartz sand, SiO2≥99.5wt%; The particle size of ordinary quartz sand is 83-106 microns; 99.5wt%>SiO2≥95wt% in ordinary quartz sand; The particle size of low-grade quartz sand is less than 83 microns; in low-grade quartz, 95wt%>SiO2≥90wt%.
3. A method for preparing quartz sand pellets as claimed in any one of claims 1 to 2, characterized in that; The steps include: Step 1, firstly crushing high-purity quartz sand, ordinary quartz sand and low-grade quartz sand into particles of required particle size; wherein the particle size of high-purity quartz sand is 106-180 microns, the particle size of ordinary quartz sand is 83-105 microns, and the particle size of low-grade quartz sand is less than 83 microns; Step 2, first add 5wt% to 6wt% of water and 1.4 to 1.6wt% of a binder to the high-purity quartz sand, and stir evenly to obtain a mixture A; Step 3, adding ordinary quartz sand to the mixture A of step 2, and then adding 5wt% to 6wt.% of water and 1.4 to 1.6wt.% of a binder relative to the mass of the ordinary quartz sand; stirring evenly to obtain a mixture B; Step 4, adding low-grade quartz sand to the mixture B of step 3, and then adding 5wt% to 6wt.% of water and 1.4 to 1.6wt.% of a binder relative to the mass of the low-grade quartz sand; stirring evenly to obtain a mixture C; Step 5, putting the mixed material C stirred evenly in step 4 into a mold, pressing it into a ball, and putting it into a drying oven at 80-120°C for drying for 3-5 hours; in an air-tight condition, low-temperature calcining the formed agglomerate at a temperature greater than or equal to 1750°C, keeping it warm for 4-6 hours, and cooling it to room temperature with the furnace to obtain quartz sand pellets for industrial silicon.
4. The method for preparing quartz sand pellets according to claim 3, characterized in that: When the particle size of high-purity quartz sand is 150-180 microns, the particle size of ordinary quartz sand is 106-125 microns, and the particle size of low-grade quartz sand is 83-90 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:
10.
5. The method for preparing quartz sand pellets according to claim 3, characterized in that: When the particle size of high-purity quartz sand is greater than or equal to 125 microns and less than 150 microns, the particle size of ordinary quartz sand is greater than or equal to 96 microns and less than 106 microns, and the particle size of low-grade quartz sand is 75-80 microns, the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 45:25:
15.
6. The method for preparing quartz sand pellets according to claim 3, characterized in that: The particle size of high-purity quartz sand is greater than or equal to 109 microns and less than 125 microns, the particle size of ordinary quartz sand is greater than or equal to 80 microns and less than 96 microns, and the particle size of low-grade quartz sand is 50-75 microns; the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40:30:
20.
7. The method for preparing quartz sand pellets according to claim 3, characterized in that: The binder in step 2, step 3 and step 4 is an organic-inorganic composite binder, in which the inorganic binder accounts for 9.5-21wt.%, and the organic binder accounts for 79-90.5wt.%; the inorganic binder is selected from water glass; and the organic binder is selected from microcrystalline cellulose.
8. The method for preparing quartz sand pellets according to claim 7, characterized in that: When the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 40:30:20, or When the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 50:20:10, The binder in step 2, step 3 and step 4 is an organic-inorganic composite binder, in which the inorganic binder accounts for 19.5-20.5wt% and the organic binder accounts for 79.5-80.5wt%; the inorganic binder is selected from water glass; the organic binder is selected from microcrystalline cellulose; When the mass ratio of high-purity quartz sand, ordinary quartz sand and low-grade quartz sand is 45:25:15, The binder in step 2, step 3 and step 4 is an organic-inorganic composite binder, in which the inorganic binder accounts for 10-10.5wt% and the organic binder accounts for 90.5-90wt%; the inorganic binder is selected from water glass; and the organic binder is selected from microcrystalline cellulose.
9. The method for preparing quartz sand pellets according to claim 3, characterized in that: The diameter of the obtained quartz sand pellets for industrial silicon is 50 to 60 mm.
10. An application of the quartz sand pellets as claimed in any one of claims 1 to 2, characterized in that: The method comprises mixing quartz sand pellets and a carbonaceous reducing agent in a mass ratio of quartz sand pellets: carbonaceous reducing agent = 0.95-1.05:0.95-1.1, preferably 0.95-1:1-1.05, uniformly, and then adding the mixture into a submerged arc furnace for smelting at a temperature of 2000-2300 degrees Celsius to obtain industrial silicon.
Citation Information
Patent Citations
Method for smelting industrial silicon by mixing quartz sand and quartz stone
CN116873931A
Method for preparing pellets by coating silica particles with different binding coals for industrial silicon
CN116282032A
Quartz carbon-iron pellet for producing high-purity silicon iron and preparation method of quartz carbon-iron pellet
CN117778715A
High density fused silica process and product
US5096865A