High-purity silica sol for polishing monocrystalline silicon substrate and preparation method of high-purity silica sol
Through dilute hydrochloric acid soaking and acid-base treatment combined with chelating agent adjustment, the preparation process of high-purity silica sol is simplified, the impurity control problem in the prior art is solved, and the production of silica sol with high purity and good polishing effect is achieved.
Patent Information
- Application Number
- CN202411106184.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
AI Technical Summary
There is room for improvement in the existing high-purity silicon sol preparation methods, especially when using water glass and hydrolyzable organosilane as raw materials, the preparation process is complicated and impurity control is difficult to achieve high purity.
The cation exchange resin column was soaked in dilute hydrochloric acid, combined with low-degree water glass and alkaline solution treatment, and added surfactant and complexing agent, and purified by acid-base regulation and chelating agent to achieve the preparation of high-purity silica sol.
The preparation process is simplified, the purity and polishing effect of the silicon sol are improved, and the operation is convenient, and the impurity concentration can be effectively controlled to obtain a high-purity silicon sol.
Smart Images

Figure CN118877901A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor processing, and in particular to a high-purity silica sol used for polishing a single-crystal silicon substrate and a preparation method thereof. Background Art
[0002] Silica sol is a colloidal dispersion in which nano-SiO2 particles are uniformly dispersed in water or organic solvents, also known as silicic acid solution. It is often a colorless or milky white transparent liquid with a large specific surface area and high adsorption. Its high dispersibility, high fire resistance and thermal insulation, as well as its odorless and non-toxic properties make it extremely safe in many application scenarios. Silica sol can be used as an adsorbent, separation agent and catalyst, and has good chemical stability and high temperature stability. High-purity silica sol can be used to improve certain properties of polishing liquids and special coatings.
[0003] The silica particles in silica sol are reactive and can be used in various industries, including coatings, precision casting, papermaking, textiles, and electronics. However, ordinary silica sol contains alkali metal ion impurities such as sodium and potassium, so the concentration of these ions needs to be controlled, generally below 10ppm, to obtain high-purity silica sol.
[0004] As a new type of semiconductor material, silicon carbide has the advantages of large bandgap, high breakdown electric field, high thermal conductivity and high saturated electron drift rate, which can meet the needs of high-frequency and high-power electronic devices. Therefore, the application of silicon carbide in electronic components has become an inevitable trend of future development, and the growth technology of silicon carbide is the prerequisite for device manufacturing. In this process, large-particle silica sol can play a good role as a polishing agent for single crystal silicon, and the polishing speed is fast.
[0005] At present, the existing preparation process combines the peptization method, ion exchange method and elemental silicon dissolution method to obtain highly uniformly distributed and highly concentrated silica sol. In addition, the preparation method of high-purity silica sol includes synthesis using water glass as raw material and using hydrolyzable organic silane as raw material, and there is still room for improvement in its preparation process. Summary of the invention
[0006] In the prior art, the preparation method of high-purity silica sol includes synthesis using water glass as raw material and using hydrolyzable organic silane as raw material. There is still room for improvement in the preparation process. Therefore, the present invention provides a high-purity silica sol for polishing single crystal silicon substrates and a preparation method thereof to solve the above problems.
[0007] In a first aspect, the present invention provides a method for preparing a high-purity silica sol for polishing a single crystal silicon substrate, which comprises the following steps: S1, soaking the cation exchange resin column with dilute hydrochloric acid solution for 20-40 minutes, washing with clean water until the pH of the discharged solution is 7, and obtaining a cation resin treatment solution; S2. Slowly adding a low-concentration water glass solution to the cation exchange resin column under stirring to obtain a new silicic acid solution having a pH value of 4-5 at room temperature; S3, adding alkaline solution and the new silicic acid solution into the reaction kettle in sequence, raising the temperature to 97-99° C. to obtain a pH value of 12-15 for the solution in the kettle; S4, adding surfactant and complexing agent to the solution in the kettle, while continuing to drop sodium hydroxide solution to adjust the pH value to 9-10, stopping adding the new silicate solution and then heating and keeping warm; S5, placing the solution in a pool for ventilation and cooling, and filtering; S6. Purify the filtered solution and add a chelating agent for adjustment to obtain a high-purity silica sol.
[0008] In one implementation, in S1, the concentration of the dilute hydrochloric acid is 0.1-0.5 mol / L, and the soaking time of the dilute hydrochloric acid is 25-30 min.
[0009] In one implementation, in S2, the flow rate through the cation exchange resin column is 10-30 L / min.
[0010] In one implementation, in S2, the mass content of SiO2 in the low-concentration water glass solution is 20%, the mass content of Na2O is 5-6%, and the pH value of the new silicic acid solution is 4.5.
[0011] In one implementation, in S3, specifically including: adding sodium hydroxide solution when the temperature is raised to 75°C; adding the new silicic acid solution after the temperature in the reactor is raised to 85°C, and keeping the temperature for 25-35 minutes when the pH value is 12-15.
[0012] In one implementation, in S4, the surfactant is one or more of polyacrylic acid and its salts, alkylbenzene sulfonic acid and its salts, alkyl sulfates, alkyl ammonium chloride and alkylphenol polyoxyethylene ether; the complexing agent is one or more of hydroxyethylidene diphosphonic acid and its salts, ethylenediaminetetraacetic acid and its salts, oxalic acid, glycine, ascorbic acid, citric acid, potassium pyrophosphate and potassium thiosulfate.
[0013] In one implementation, in S5, a filter element made of PFA material is used for filtering, two-stage or three-stage filtration is adopted, and the filtration accuracy is 0.2 μm-5 μm.
[0014] In one implementation, in S6, specifically including: controlling the temperature of the silica sol at 0-60°C, countercurrently passing through a strong acid cation exchange bed; then countercurrently passing through a strong base anion exchange bed, with a flow rate of 1-20 m / h during countercurrent; adding a chelating agent to adjust the pH of the silica sol to 1.0-3.0; then countercurrently passing through a mixed bed of strong acid and strong base ion exchange resins, with a flow rate of 1-20 m / h during countercurrent, to obtain purified silica sol.
[0015] In one implementation, in S6, the chelating agent is a phosphonic acid-based chelating agent.
[0016] In a second aspect, the present invention further provides a high-purity silica sol for polishing a single-crystal silicon substrate, which is prepared by using the high-purity silica sol for polishing a single-crystal silicon substrate mentioned above.
[0017] Beneficial effects: The method for preparing high-purity silica sol for polishing single-crystal silicon substrates provided by the present invention combines the processes of ion exchange, acid-base treatment and chelating agent adjustment. The preparation process is simple and easy to operate, and silica sol with high purity and good polishing effect can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The present invention is a flowchart of the steps of preparing a method for high-purity silica sol for polishing a single-crystal silicon substrate.
[0019] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the description of the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" described below means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms is not necessarily for the same embodiment or example. Moreover, the technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.
[0021] Specific reference Figure 1 , Figure 1 The present invention provides a method for preparing a high-purity silica sol for polishing a single-crystal silicon substrate, which comprises the following steps: S1, soaking the cation exchange resin column with dilute hydrochloric acid solution for 20-40 minutes, washing with clean water until the pH of the discharged solution is 7, and obtaining a cation resin treatment solution; S2. Slowly adding a low-concentration water glass solution to the cation exchange resin column under stirring to obtain a new silicic acid solution having a pH value of 4-5 at room temperature; S3, adding alkaline solution and the new silicic acid solution into the reaction kettle in sequence, raising the temperature to 97-99° C. to obtain a pH value of 12-15 for the solution in the kettle; S4, adding surfactant and complexing agent to the solution in the kettle, while continuing to drop sodium hydroxide solution to adjust the pH value to 9-10, stopping adding the new silicate solution and then heating and keeping warm; S5, placing the solution in a pool for ventilation and cooling, and filtering; S6. Purify the filtered solution and add a chelating agent for adjustment to obtain a high-purity silica sol.
[0022] Specifically, in S1, the concentration of the dilute hydrochloric acid is 0.1-0.5 mol / L, and the dilute hydrochloric acid soaking time is 25-30 min. Preferably, the mass concentration of the dilute hydrochloric acid is 0.3 mol / L, and the dilute hydrochloric acid soaking time is 30 min. In this step, the concentration and time of soaking the cation exchange resin column with dilute hydrochloric acid can be adjusted to better remove impurities on the resin and improve the purity of the prepared silica sol.
[0023] Specifically, in S2, the flow rate through the cation exchange resin column is 10-30 L / min. By adjusting the flow rate through the column, the low-concentration water glass solution can be more effectively added to the cation exchange resin column, thereby improving the preparation efficiency of the new silicic acid solution.
[0024] Specifically, in S2, the mass content of SiO2 in the low-density water glass solution is 20%, the mass content of Na2O is 5-6%, and the pH value of the newly formed silicic acid solution is 4.5. In this step, by controlling the mass content of SiO2 and Na2O in the low-density water glass solution and the pH value of the newly formed silicic acid solution, the composition and quality of the silica sol can be better controlled. Furthermore, the alkaline solution and the newly formed silicic acid solution are added under stirring.
[0025] Specifically, in S3, it specifically includes: adding sodium hydroxide solution when the temperature is raised to 75°C; adding the new silicic acid solution after heating the reactor to 85°C, and keeping warm for 25 to 35 minutes when the pH is 12 to 15. By controlling the time, temperature and pH value of adding alkaline solution and new silicic acid solution, a high-purity silica sol with ideal composition and performance can be obtained. In other embodiments, other alkaline substances can also be used instead of sodium hydroxide solution to seek more efficient reaction conditions and higher purity silica sol. The alkaline substance is one or more of potassium hydroxide, ammonia water, ethylenediamine, propylenediamine, hexamethylenediamine, and tetramethylammonium hydroxide.
[0026] Specifically, in S4, the surfactant is one or more of polyacrylic acid and its salts, alkylbenzene sulfonic acid and its salts, alkyl sulfate, alkyl ammonium chloride and alkylphenol polyoxyethylene ether; the complexing agent is one or more of hydroxyethylidene diphosphonic acid and its salts, ethylenediaminetetraacetic acid and its salts, oxalic acid, glycine, ascorbic acid, citric acid, potassium pyrophosphate and potassium thiosulfate. Appropriate selection of the surfactant and complexing agent and control of the dripping speed and time of the sodium hydroxide solution can improve the stability and polishing effect of the silica sol. In other embodiments, the addition speed and ratio of the new silicic acid solution and the sodium hydroxide solution can be optimized to achieve more accurate pH adjustment and better product quality control.
[0027] Specifically, in S5, a filter element made of PFA material is used for filtration, and two-stage or three-stage filtration is used, with a filtration accuracy of 0.2 μm-5 μm. The use of a filter element made of PFA material and two-stage or three-stage filtration can effectively remove impurities in the silica sol and ensure the purity of the silica sol. Furthermore, the present invention can also use an ultrafilter for ultrafiltration.
[0028] Specifically, in S6, it specifically includes: controlling the temperature of the silica sol at 0-60°C, countercurrently passing through a strong acid cation exchange bed; then countercurrently passing through a strong base anion exchange bed, and the flow rate of the liquid during countercurrent is 1-20 m / h; adding a chelating agent to make the pH of the silica sol 1.0-3.0; then countercurrently passing through a mixed bed of strong acid and strong base ion exchange resins, and the flow rate of the liquid during countercurrent is 1-20 m / h, to obtain purified silica sol. In this step, by countercurrently passing through a strong acid cation exchange bed and a strong base anion exchange bed, and adding a chelating agent and then countercurrently passing through a mixed bed of strong acid and strong base ion exchange resins, a more purified silica sol can be obtained. Furthermore, in this step, processes such as membrane separation and / or ion exchange can also be introduced to further improve the purity and stability of the ultra-high purity silica sol.
[0029] In S6, preferably, the chelating agent is a phosphonic acid chelating agent. The use of a phosphonic acid chelating agent can better adjust the pH value of the silica sol and improve the stability and polishing effect of the silica sol.
[0030] In summary, the method for preparing high-purity silica sol for polishing single-crystal silicon substrates provided by the present invention combines the processes of ion exchange, acid-base treatment and chelating agent adjustment. The preparation process is simple and easy to operate, and silica sol with high purity and good polishing effect can be obtained.
[0031] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing high-purity silica sol for polishing single crystal silicon substrates, characterized in that: The following steps are involved: S1, soaking the cation exchange resin column with dilute hydrochloric acid solution for 20-40 minutes, washing with clean water until the pH of the discharged solution is 7, and obtaining a cation resin treatment solution; S2. Slowly adding a low-concentration water glass solution to the cation exchange resin column under stirring to obtain a new silicic acid solution having a pH value of 4-5 at room temperature; S3, adding alkaline solution and the new silicic acid solution into the reaction kettle in sequence, raising the temperature to 97-99° C. to obtain a pH value of 12-15 for the solution in the kettle; S4, adding surfactant and complexing agent to the solution in the kettle, while continuing to drop sodium hydroxide solution to adjust the pH value to 9-10, stopping adding the new silicate solution and then heating and keeping warm; S5, placing the solution in a pool for ventilation and cooling, and filtering; S6. Purify the filtered solution and add a chelating agent for adjustment to obtain a high-purity silica sol.
2. The method for preparing high-purity silica sol for polishing single crystal silicon substrates according to claim 1, characterized in that: In S1, the concentration of the dilute hydrochloric acid is 0.1-0.5 mol / L, and the soaking time of the dilute hydrochloric acid is 25-30 min.
3. The method for preparing high-purity silica sol for polishing single crystal silicon substrate according to claim 1, characterized in that: In S2, the flow rate through the cation exchange resin column is 10-30 L / min.
4. The method for preparing high-purity silica sol for polishing single crystal silicon substrate according to claim 1, characterized in that: In S2, the mass content of SiO2 in the low-concentration water glass solution is 20%, the mass content of Na2O is 5-6%, and the pH value of the new silicic acid solution is 4.
5.
5. The method for preparing high-purity silica sol for polishing single crystal silicon substrate according to claim 1, characterized in that: In S3, specifically, the steps include: adding sodium hydroxide solution when the temperature reaches 75°C; and adding the new silicic acid solution after the temperature in the reactor is increased to 85°C, and keeping the temperature for 25-35 minutes when the pH value reaches 12-15.
6. The method for preparing high-purity silica sol for polishing single crystal silicon substrates according to claim 1, characterized in that: In S4, the surfactant is one or more of polyacrylic acid and its salts, alkylbenzene sulfonic acid and its salts, alkyl sulfates, alkyl ammonium chloride and alkylphenol polyoxyethylene ether; the complexing agent is one or more of hydroxyethylidene diphosphonic acid and its salts, ethylenediaminetetraacetic acid and its salts, oxalic acid, glycine, ascorbic acid, citric acid, potassium pyrophosphate and potassium thiosulfate.
7. The method for preparing high-purity silica sol for polishing single crystal silicon substrate according to claim 1, characterized in that: In S5, the filter uses a PFA filter element, with two-stage or three-stage filtration and a filtration accuracy of 0.2μm-5μm.
8. The method for preparing high-purity silica sol for polishing single crystal silicon substrates according to claim 1, characterized in that: In S6, it specifically includes: controlling the temperature of the silica sol at 0-60°C, countercurrently passing through a strong acid cation exchange bed; countercurrently passing through a strong base anion exchange bed, and the flow rate of the liquid in the countercurrent state is 1-20 m / h; adding a chelating agent to adjust the pH of the silica sol to 1.0-3.0; countercurrently passing through a mixed bed of strong acid and strong base ion exchange resins, and the flow rate of the liquid in the countercurrent state is 1-20 m / h, to obtain purified silica sol.
9. The method for preparing high-purity silica sol for polishing single crystal silicon substrates according to claim 8, characterized in that: In S6, the chelating agent is a phosphonic acid-based chelating agent.
10. A high-purity silica sol for polishing a single-crystal silicon substrate, characterized in that: The method is prepared by using the high-purity silica sol for polishing a single crystal silicon substrate as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Purification method of ultra-pure silicon dioxide sol
CN101475180A
Industrial silicon sol preparation method
CN106115721A
Silica sol with ultralow dispersion coefficient as well as preparation method and application thereof
CN115353806A
Nodular Silica Sol and Method of Producing the Same
US20100146864A1