Preparation method of titanium liquid hydrolysis and seed crystal addition
By using sodium dodecylbenzenesulfonate and carboxypropyl methylcellulose to replace liquid alkali, the problems of high cost and wide particle size distribution in hydrolysis of titanium liquid and hydrolysis plus seed crystal preparation are solved, and lower cost and narrower Effect of particle size distribution.
Patent Information
- Application Number
- CN202411165302.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-01
AI Technical Summary
The existing titanium liquid hydrolysis plus seed crystal preparation methods use liquid alkali to cause high cost and wide particle size distribution, and complex process.
Sodium dodecylbenzenesulfonate and carboxypropylmethylcellulose replace liquid alkali, seed crystals are prepared through specific ratios and process steps, promoting the hydrolysis of titanium liquid and the formation of seed crystals, and forming an adsorption layer to enhance the particles. Stability and dispersion.
The production cost is reduced, and the resulting metatitanic acid particle size distribution is narrow, which improves the stability and dispersion of particles and simplifies the process flow.
Smart Images

Figure CN118877934A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium dioxide production, in particular to a method for preparing titanium liquid by hydrolyzing and adding crystal seeds. Background Art
[0002] In the production process of titanium dioxide by sulfuric acid method, titanium dioxide uses the hydrolysis product metatitanic acid as a precursor, which is converted into the required TiO2 coating after washing and calcination. The properties of the metatitanic acid precursor obtained by hydrolysis determine the performance of the coating. Hydrolysis is the core technology of titanium dioxide production by sulfuric acid method. At present, the main hydrolysis methods used in industry are self-generated seed method and external seed method. The external seed method was successfully developed by McBollon in 1930. It mainly uses ammonia water or sodium hydroxide to react with part of the titanium liquid to neutralize and cultivate a certain number of good seeds with composition before hydrolysis. The seeds prepared by chemical method are added to titanium liquid under certain conditions to induce hydrolysis reaction. If the grains prepared by the seeds are uniform, the supersaturation in the hydrolysis process can be effectively controlled to obtain a product with better grain distribution. The external seed method is simple to operate and is suitable for direct hydrolysis of low-concentration titanium liquid to obtain titanium dioxide with excellent pigment performance. However, the process of chemical exogenous seeding reduces the purity of the product due to the introduction of external elements, which is easy to affect the quality of the final pigment. The existing external seeding process generally uses liquid caustic soda, which has high cost and wide distribution of seed crystals.
[0003] Chinese invention patent announcement number CN105502483B discloses a method for preparing rutile titanium dioxide with microwave assistance, which uses microwave heating activation to prepare seeds with high hydrolysis activity. The seeds are used to hydrolyze industrial titanium liquid with external seeds to prepare metatitanic acid. The hydrolysis product metatitanic acid is calcined at a lower temperature to obtain rutile titanium dioxide. The seed preparation process used in this method is complicated, and the particle size distribution of the prepared metatitanic acid cannot be seen. Summary of the invention
[0004] The technical problem to be solved by the present invention is that the existing method for preparing titanium liquid hydrolyzed additional crystal seeds uses liquid alkali, resulting in high cost, wide particle size distribution, or complex seed production process. Therefore, a method for preparing titanium liquid hydrolyzed additional crystal seeds is provided.
[0005] The technical solution of the present invention is: a method for preparing titanium liquid by hydrolysis and adding crystal seeds, comprising the following steps:
[0006] (1) Raise the temperature of the titanium dioxide seed liquid with a titanium dioxide concentration of 170-200 g / L to 86°C-92°C; (2) Dissolve a certain proportion of sodium dodecylbenzene sulfonate and carboxypropyl methylcellulose in water to form a mixed solution; (3) Select an appropriate amount of mixed solution according to the titanium dioxide concentration of the titanium dioxide seed liquid so that the titanium dioxide concentration of the mixed seed crystals is between 130 g / L-140 g / L, and raise the temperature of the mixed solution to 86°C-92°C; (4) Add the titanium dioxide seed liquid that has been heated in step (1) into the mixed solution and keep it in the mixture within 5 min-7 min. After the mixture is completely heated, raise the temperature to 95°C-98°C to complete the seed crystal preparation.
[0007] In the above scheme, the ratio of the amount of sodium dodecylbenzene sulfonate added to the amount of titanium liquid converted to titanium is 1: (4-6.5), and the amount of carboxypropyl methylcellulose added is 0.5 kg / m 3 -0.9kg / m 3 .
[0008] The improvement of the above scheme is that it also includes step (5), taking 10 ml of the prepared seed crystals, adding them to a 500 ml conical flask, slowly adding distilled water at room temperature, and shaking quickly. If no turbidity appears, continue to add distilled water until turbidity appears, immediately stop adding water, and observe the amount of distilled water added, which is recorded as the stability of the seed crystals.
[0009] The invention has the beneficial effects of using sodium dodecylbenzene sulfonate and carboxypropyl methylcellulose to replace liquid alkali, thereby reducing the production cost, and at the same time, the obtained metatitanic acid particle size is narrower than that of the seed crystal prepared by using liquid alkali; the function of carboxypropyl methylcellulose (HPMC) is mainly reflected in that it can act with hydrogen bonds or other interaction forces on the surface of particles to form an adsorption layer to keep the particles in a dispersed state, and can also form a spatial arrangement of a network structure through its high molecular weight and soft chain structure to further enhance the stability of the particles; the weak alkalinity of sodium dodecylbenzene sulfonate can neutralize the pH of titanium liquid, promote the hydrolysis of titanium liquid and the formation of seed crystals, and as a surfactant, it can effectively promote the interaction between molecules, which is conducive to the induction of the subsequent hydrolysis process. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is a particle size distribution diagram of Example 1 of the present invention;
[0011] Figure 2 is a particle size distribution diagram of Example 2 of the present invention;
[0012] Figure 3 is a particle size distribution diagram of Example 3 of the present invention;
[0013] Figure 4 is a particle size distribution diagram of Example 4 of the present invention;
[0014] Figure 5 is a particle size distribution diagram of Comparative Example 1 of the present invention;
[0015] Figure 6 is a particle size distribution diagram of Comparative Example 2 of the present invention;
[0016] Figure 7 It is the particle size distribution diagram of Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0017] The present invention will be further described below in conjunction with the embodiments and drawings.
[0018] like Figure 1-7 As shown, Example 1:
[0019] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 191 g / L to 87°C. The volume of the seed titanium liquid is 2.4% of the volume of the process titanium liquid.
[0020] 2. Dissolve sodium dodecylbenzene sulfonate (the ratio of sodium dodecylbenzene sulfonate to titanium liquid is 1:5.2) in water; at the same time, add carboxypropyl methylcellulose (the amount is 0.7 kg / m 3 ) dissolved in water.
[0021] 3. Add a certain amount of mixed liquid (calculated according to the titanium dioxide concentration of the seed titanium liquid) into the seed crystal preparation tank and raise the temperature to 88°C.
[0022] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 100.
[0023] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0024] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0025] Embodiment 2:
[0026] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 189 g / L to 87°C. The volume of the seed titanium liquid is 2.4% of the volume of the process titanium liquid.
[0027] 2. Dissolve sodium dodecylbenzene sulfonate (the ratio of sodium dodecylbenzene sulfonate to titanium liquid is 1:4.3) in water; at the same time, add carboxypropyl methylcellulose (the amount is 0.65kg / m 3 ) dissolved in water.
[0028] 3. Add a certain amount of mixed liquid (calculated according to the titanium dioxide concentration of the seed titanium liquid) into the seed crystal preparation tank and raise the temperature to 88°C.
[0029] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 100.
[0030] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0031] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0032] Embodiment 3:
[0033] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 192 g / L to 87°C. The volume of the seed titanium liquid is 2.4% of the volume of the process titanium liquid.
[0034] 2. Dissolve sodium dodecylbenzene sulfonate (the ratio of sodium dodecylbenzene sulfonate to titanium liquid is 1:6.3) in water; at the same time, add carboxypropyl methylcellulose (the amount is 0.85 kg / m 3 ) dissolved in water.
[0035] 3. Add a certain amount of mixed liquid (calculated according to the titanium dioxide concentration of the seed titanium liquid) into the seed crystal preparation tank and raise the temperature to 88°C.
[0036] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 95.
[0037] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0038] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0039] Embodiment 4:
[0040] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 190 g / L to 87°C. The volume of the seed titanium liquid is 2.0% of the volume of the process titanium liquid.
[0041] 2. Dissolve sodium dodecylbenzene sulfonate (the ratio of sodium dodecylbenzene sulfonate to titanium liquid is 1:5.2) in water; at the same time, add carboxypropyl methylcellulose (the amount is 0.7 kg / m 3 ) dissolved in water.
[0042] 3. Add a certain amount of mixed liquid (calculated according to the titanium dioxide concentration of the seed titanium liquid) into the seed crystal preparation tank and raise the temperature to 88°C.
[0043] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 110.
[0044] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0045] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0046] Comparative Example 1:
[0047] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 191 g / L to 87°C. The volume of the seed titanium liquid is 2.4% of the volume of the process titanium liquid.
[0048] 2. Dissolve sodium dodecylbenzene sulfonate (the ratio of sodium dodecylbenzene sulfonate to titanium seed liquid is 1:5.2) in water.
[0049] 3. Add a certain amount of mixed liquid (calculated according to the titanium dioxide concentration of the seed titanium liquid) into the seed crystal preparation tank and raise the temperature to 88°C.
[0050] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 100.
[0051] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0052] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0053] Comparative Example 2:
[0054] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 191 g / L to 87°C. The volume of the seed titanium liquid is 2.4% of the volume of the process titanium liquid.
[0055] 2. Use 9.2% liquid caustic soda and dissolve carboxypropyl methylcellulose (0.7kg / m3) in the liquid caustic soda solution.
[0056] 3. Add a quantitative amount of liquid alkali mixed solution (based on the alkali-titanium ratio of 0.15:1) into the seed preparation tank and heat it to 88°C.
[0057] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 100.
[0058] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0059] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0060] Comparative Example 3:
[0061] 1. Raise the temperature of the seed titanium liquid with a titanium dioxide concentration of 193 g / L to 87°C. The volume of the seed titanium liquid is 2.4% of the volume of the process titanium liquid.
[0062] 2. Use liquid caustic soda at a concentration of 9.2%.
[0063] 3. Add a quantitative amount of liquid alkali solution (based on the alkali-titanium ratio of 0.15:1) into the seed preparation tank and heat it to 88°C.
[0064] 4. Put the titanium seed liquid after heating into the mixed liquid and keep it in 5-7 minutes. After the temperature is raised to 97℃, the stability is measured at 100.
[0065] 5. Place the seed crystal into the preheated industrial titanium liquid, stir for 15 minutes, and place it into the hydrolysis pot to start the hydrolysis operation.
[0066] 6. After the hydrolysis is completed, the particle size of the metatitanic acid after hydrolysis is detected.
[0067] The particle size distribution data of Examples 1 to 4 and Comparative Examples 1 to 3 are as follows:
[0068] Sample name D10(um) D50(um) D90(um) (D90-D10) / D50 Example 1 0.712 2.156 3.532 1.308 Example 2 0.723 2.286 3.897 1.388 Example 3 0.72 2.233 3.797 1.378 Example 4 0.537 2.04 3.547 1.475 Comparative Example 1 0.544 1.996 3.489 1.475 Comparative Example 2 0.427 2.134 3.85 1.604 Comparative Example 3 0.428 2.253 4.054 1.609
[0069] Wherein (D90-D10) / D50 reflects the distribution of particle size, and the smaller its value is, the narrower the particle size distribution is. It can be seen from Comparative Examples 2 and 3 that when liquid alkali is used to prepare the added seed, the hydrolysis particle size distribution is obviously the widest. It can be seen from Example 1 and Comparative Example 1 that the particle size distribution can be obviously narrowed after using carboxypropyl methylcellulose. It can be seen from Example 1, Example 2 and Example 3 that different amounts of sodium dodecylbenzene sulfonate and carboxypropyl methylcellulose have a certain effect on the particle size distribution, and the more the amount is added within a certain range, the narrower the particle size distribution is.
Claims
1. A method for preparing titanium liquid by hydrolysis and adding seed crystals, characterized in that: The following steps are involved: (1) Raise the temperature of the titanium dioxide seed liquid with a titanium dioxide concentration of 170-200 g / L to 86°C-92°C; (2) Dissolve a certain proportion of sodium dodecylbenzene sulfonate and carboxypropyl methylcellulose in water to form a mixed solution; (3) Select an appropriate amount of mixed solution according to the titanium dioxide concentration of the titanium dioxide seed liquid so that the titanium dioxide concentration of the mixed seed crystals is between 130 g / L-140 g / L, and raise the temperature of the mixed solution to 86°C-92°C; (4) Add the titanium dioxide seed liquid that has been heated in step (1) into the mixed solution and keep it in the mixture within 5 min-7 min. After the mixture is completely heated, raise the temperature to 95°C-98°C to complete the seed crystal preparation.
2. The method for preparing titanium liquid by hydrolysis and adding seed crystals as claimed in claim 1, characterized in that: In the step (2), the ratio of the amount of sodium dodecylbenzene sulfonate added to the amount of titanium liquid converted to titanium is 1: (4-6.5), and the amount of carboxypropyl methylcellulose added is 0.5 kg / m 3 -0.9kg / m 3 .
3. The method for preparing titanium liquid by hydrolysis and adding seed crystals as claimed in claim 1, characterized in that: The method further comprises step (5), taking 10 ml of the prepared seed crystals, adding the prepared seed crystals into a 500 ml conical flask, slowly adding distilled water at room temperature, and quickly shaking the mixture. If the mixture is not turbid, continue adding distilled water until turbidity occurs, immediately stop adding water, and observe the amount of distilled water added, which is recorded as the stability of the seed crystals.