Method for recovering metal elements in waste ternary lithium battery through mechanochemical driving eutectic solvent

Through the combination technology of mechanochemical driven eutectic solvent and mesoporous microsphere aid, the problems of low leaching efficiency and pollutant emissions in lithium battery recycling are solved, and efficient and green metal elements are achieved, with a leaching rate of 90%. above.

CN118877949APending Publication Date: 2024-11-01JINAN UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410861891.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing lithium battery recycling technology has problems such as low leaching efficiency, pollutant emissions and strong acid use, which limits the sustainable recycling of used lithium batteries.

Method used

The combination technology of mechanochemical driven eutectic solvent and mesoporous microsphere aid is used to leaching and graded precipitation through the ball milling process to recover metal elements in waste ternary lithium batteries, improving leaching efficiency and reducing toxic gas emissions.

Benefits of technology

The efficient recycling of metal elements in waste lithium batteries has been achieved, with a leaching rate of more than 90%. The use of green solvents has avoided toxic gas emissions, significantly improving recycling efficiency and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877949A_ABST
    Figure CN118877949A_ABST
Patent Text Reader

Abstract

The invention provides a method for recycling metal elements in a waste ternary lithium battery by driving a eutectic solvent through mechanochemistry, which comprises the following steps: ball-milling a positive electrode material, the eutectic solvent and a grinding aid (mesoporous (alpha-SiO2.H2O) x. (Al2O3) y microspheres, x = 0.1-0.9, and y = 1-x) under the action of a ball-milling medium to obtain a leaching solution containing metal ions such as Li, Mn, Co, Ni and the like, and precipitating and calcining the leachate for multiple times, so that metal elements in the leachate are recycled in the form of metal oxides and metal carbonates. Compared with an existing heating or ball milling method, a grinding aid is further added, and the leaching efficiency is greatly improved; according to the method, the eutectic solvent is adopted as the leaching solvent, compared with traditional inorganic acid, toxic and harmful gas cannot be generated in the leaching process, the leaching efficiency is higher, and a new technical scheme is provided for green and efficient recovery of the waste ternary lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of recycling waste ternary lithium batteries, and more specifically, to a method for recovering metal elements in positive electrode materials by using a mechanochemically driven eutectic solvent. Background Art

[0002] Lithium batteries are a common energy storage unit. Compared with other types of batteries, lithium batteries can store more energy with a smaller mass, and have higher energy conversion efficiency and better high temperature resistance. However, the price fluctuations and supply shortages of metals and raw materials required for lithium battery production have severely restricted the sustainable development of the lithium battery industry. Therefore, the recycling and reuse of waste lithium batteries has become a problem that needs to be solved urgently.

[0003] At present, lithium battery recycling technology is dominated by pyrometallurgy and hydrometallurgy. The most mature recycling technology is to use pyrometallurgy and hydrometallurgy to smelt and then recover metals from the resulting alloy. In the pyrometallurgical process, in addition to obtaining the target products (such as valuable metals and graphite), pyrolysis intermediates are also produced. Although the emission of pyrolysis gases (such as SOx, Cl2 and NOx) has received increasing attention, new pollutants have also been found in the pyrolysis intermediates of the pyrometallurgical process. Compared with the pyrometallurgical process, the hydrometallurgical process has been very mature in the recycling of waste lithium batteries. Leaching and purification in the hydrometallurgical process have various advantages, including high recovery efficiency, high selectivity, low energy consumption and low gas emissions. However, from the perspective of sustainable development, the use of strong acids and the treatment of liquid waste have become major challenges at present. Therefore, there is a great need to develop a green and efficient technology for recycling waste lithium batteries.

[0004] The prior art discloses a method for recycling waste lithium batteries, which uses a eutectic solvent to leach metal elements in waste lithium batteries under heating conditions or with the assistance of ball milling to achieve the recovery of metal elements in waste lithium batteries. However, the leaching efficiency of the prior art is still low. Summary of the invention

[0005] The present invention aims to overcome the shortcomings of traditional methods for recycling waste lithium batteries, and provide a method for recovering metal elements in waste ternary lithium batteries by mechanochemically driven eutectic solvents, thereby achieving green and efficient recycling of waste ternary lithium batteries.

[0006] Therefore, the primary purpose of the present invention is a method for recovering metal elements in waste ternary lithium batteries by mechanochemically driven eutectic solvents.

[0007] To achieve the above object, the present invention adopts the following technical solutions: The present invention protects a method for recovering metal elements in waste ternary lithium batteries by mechanochemically driven eutectic solvent, which is characterized by comprising the following steps: S1. Leaching: The mixture of the cathode material powder of the waste ternary lithium battery, the eutectic solvent and the grinding aid is ball-milled under the action of a ball-milling medium to obtain a leachate; S2 precipitation: the leachate was subjected to graded precipitation to obtain Ni, Co, Mn hydroxide and Li2CO3; The grinding aid is (α-SiO2·H2O) x ·(Al2O3) y Mesoporous microspheres, where x=0.1-0.9, y=1-x.

[0008] The present invention adds (α-SiO2·H2O) during the ball milling process. x ·(Al2O3) y Mesoporous microspheres are used as grinding aids. They are colorless, odorless, non-toxic, highly chemically stable, and insulating and high-temperature resistant. They have the function of network regulation, which can intensify the destruction of battery powder lattice particles and greatly improve the leaching efficiency of metal elements.

[0009] Preferably, the amount of grinding aid added in step S1 is 60 mg to 150 mg. Further preferably, the amount of grinding aid added in step S1 is 120 mg.

[0010] Preferably, the solid-to-liquid ratio of the leaching solution in step S1 is 1.0 g L -1 ~10g L -1 Preferably, the solid-to-liquid ratio of the leaching solution in step S1 is 2.5 g L -1 .

[0011] Preferably, the rotation speed of the ball mill in step S1 is 200 rpm to 600 rpm. Further preferably, the rotation speed of the ball mill in step S1 is 600 rpm.

[0012] Preferably, the ball milling time in step S1 is 30 to 120 minutes. Further preferably, the ball milling time in step S2 is 120 minutes.

[0013] Preferably, the eutectic solvent in step S1 is at least one selected from choline chloride-ethylene glycol, choline chloride-urea, choline chloride-malonic acid or choline chloride-benzoic acid.

[0014] Further preferably, the molar ratio of choline chloride to ethylene glycol, the molar ratio of choline chloride to urea, the molar ratio of choline chloride to malonic acid, and the molar ratio of choline chloride to benzoic acid are 1:1 to 3. Further preferably, the molar ratio of choline chloride to ethylene glycol, the molar ratio of choline chloride to urea, the molar ratio of choline chloride to malonic acid, the molar ratio of choline chloride to malonic acid, or the molar ratio of choline chloride to benzoic acid is 1:2.

[0015] Preferably, the ball milling medium is a steel ball. Further preferably, the mass of the steel ball is 50 g to 100 g. Further preferably, the mass of the steel ball is 60 g.

[0016] Preferably, the ball milling is carried out in a stainless steel ball milling jar. Further preferably, the capacity of the stainless steel ball milling jar is 100 mL.

[0017] Preferably, the graded precipitation in step S2 comprises the following steps: S21. Separating the first solution from the leachate, adjusting the pH value of the first solution to a pH of 9 to 12, and separating the hydroxides of Ni, Co, and Mn and a second solution; S22. Adding a soluble carbonate to the second solution to separate Li2CO3.

[0018] Preferably, the pH adjuster for adjusting the pH value of the first solution in step S21 is selected from at least one of NaOH and KOH. Further preferably, the concentration of the pH adjuster is 0.5M.

[0019] Preferably, the soluble carbonate in step S22 is selected from at least one of Na2CO3 and K2CO3. Further preferably, the concentration of the soluble carbonate is 0.5M.

[0020] Preferably, the pH in step S21 is 10.

[0021] Preferably, the recovery method further comprises the following steps: S3. Calcination: calcining the hydroxides of Ni, Co and Mn at 500-700° C. for 3-6 hours to obtain metal oxides of Ni, Co and Mn.

[0022] More preferably, the calcination temperature is 600°C.

[0023] More preferably, the calcination time is 5 hours.

[0024] Preferably, the recovery method further comprises the following steps: S0. Pretreatment: Discharge, disassemble, and crush the used ternary lithium batteries, and sort them to obtain positive electrode material powder.

[0025] Preferably, the discharge treatment in step S0 uses a homemade lighting device.

[0026] Preferably, the crushing in step S0 is performed using a high-speed universal crusher.

[0027] Preferably, the separation in step S0 includes: using a 200-mesh sieve to separate the aluminum foil and the positive electrode material powder; using deionized water as a medium and performing ultrasonic treatment in an ultrasonic device to achieve separation of the copper foil and graphite.

[0028] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention provides a method for recovering metal elements in waste ternary lithium batteries by mechanochemically driven eutectic solvent. Under the action of ball milling, the leaching rates of Li, Mn, Co and Ni in the positive electrode material can reach more than 90% after leaching in the eutectic solvent for 120 minutes. 0.5M NaOH is added to precipitate Ni, Co and Mn in the leachate in the form of Me(OH)2 (Me=Ni, Co, Mn), and then 0.5M Na2CO3 is added to recover Li in the leachate in the form of Li2CO3. The waste liquid generated is discharged after being treated to meet the standards.

[0029] 2. The present invention adopts eutectic solvent as leaching solvent. Compared with traditional inorganic acid, no toxic and harmful gases are generated during the leaching process, and the leaching efficiency is higher, which provides a new technical solution for green and efficient recycling of waste ternary lithium batteries.

[0030] 3. The present invention adds a specific grinding aid during the ball milling process, so that the leaching efficiency of Li, Mn, Co, and Ni in the eutectic solvent is as high as 99%, which greatly improves the leaching efficiency compared with the existing heating leaching or ball milling assisted method. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The XRD spectrum of the Li2CO3 obtained in Example 1 is compared with the standard card.

[0032] Figure 2 , Figure 3 The XRD spectrum of the metal oxide obtained in Example 1 is compared with the standard card. DETAILED DESCRIPTION

[0033] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.

[0034] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0035] Example 1 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods S0. Pretreatment: Discharge, disassemble, and crush the used ternary lithium batteries, and sort them to obtain positive electrode material powder.

[0036] Specifically, the waste ternary lithium battery is first completely discharged on a homemade lighting device and disassembled in a fume hood. The negative electrode, positive electrode, plastic separator, shell and other components are separated. The positive electrode is cleaned and dried, and then placed in a high-speed universal grinder for mechanical and physical crushing. A 200-mesh sieve is used to separate the aluminum foil and the positive electrode material powder. Deionized water is used as the medium, and ultrasonic treatment is performed in an ultrasonic device to achieve the separation of copper foil and graphite.

[0037] S1. Leaching: The positive electrode material, eutectic solvent, grinding aid (mesoporous (α-SiO2·H2O) x ·(Al2O3) y The microspheres (x=0.1-0.9, y=1-x)) are mixed in a certain solid-liquid ratio and added to a stainless steel ball mill, and a certain mass of steel balls are added to ball mill at a certain speed to obtain the leaching solution.

[0038] Specifically, the eutectic solvent is first prepared: choline chloride and ethylene glycol in a molar ratio of 1:2 are mixed in a beaker, and magnetic stirring is performed at 80° C. for 60 minutes. The obtained eutectic solvent is named choline chloride-ethylene glycol.

[0039] Grinding aid (mesoporous (α-SiO2·H2O) x ·(Al2O3) y Preparation of microspheres (x = 0.1-0.9, y = 1-x): The reaction was carried out in a 250 ml flask at 35 °C and magnetically stirred at 300 rpm. First, solution I containing KCl (0.0015 g), ethanol (38 ml), water (6 ml) and ammonia (3 ml) was added to a 250 mL flask and magnetically stirred at 300 rpm at 35 °C. Then, solution II containing 58 ml ethanol, 5.64 g tetraethyl orthosilicate and 5.06 g ammonium aluminum sulfate was continuously added to the flask using a syringe pump within 2 hours. After further reaction for 15 hours, the obtained microspheres were centrifuged and purified and washed with ethanol three times. Finally, the microspheres were dried under vacuum at room temperature.

[0040] Then, 0.1 g of positive electrode material powder and 120 mg of grinding aid (mesoporous (α-SiO2·H2O)) were weighed using an analytical balance. x·(Al2O3) y Microspheres (x = 0.1-0.9, y = 1-x) were physically mixed with 40 ml of choline chloride-ethylene glycol (solid-liquid ratio 2.5 g L -1 ), then added into a 100 ml stainless steel ball mill containing 60 g steel balls, and ball milled at 600 rpm for 30 min, 60 min, and 120 min to obtain an extract after the ball milling.

[0041] S2. Precipitation: The leaching solution is filtered and separated to obtain a filtrate and a filter residue. NaOH and Na2CO3 are added to the filtrate to precipitate Ni, Co, Mn and Li in the filtrate step by step.

[0042] Specifically, first slowly add deionized water to the filtrate, and when the filtrate becomes colorless, add 0.5M NaOH solution, adjust the pH of the filtrate to 10, and then stir magnetically for 30 minutes. After the reaction is completed, centrifuge to obtain a Li-containing solution and a precipitate. The precipitate is washed three times with deionized water and then dried at 60°C for 12 hours to obtain Me(OH)2 (Me=Ni, Co, Mn). The Li-containing solution is heated to 90°C in a water bath, 0.5M Na2CO3 is added, and after reacting for 60 minutes, centrifuge immediately to obtain a white precipitate Li2CO3.

[0043] S3. Calcination: Calcine Me(OH)2 (Me = Ni, Co, Mn) at 500-700°C for 3-6h to obtain metal oxides of Ni, Co, and Mn.

[0044] Specifically, Me(OH)2 (Me = Ni, Co, Mn) was calcined at 600°C for 5 h to obtain metal oxides.

[0045] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 99%.

[0046] Example 2 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as in Example 1, except that the eutectic solvent is choline chloride-urea.

[0047] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-urea for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 95%.

[0048] Example 3 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as in Example 1, except that the eutectic solvent is choline chloride-malonic acid.

[0049] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-malonic acid for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 92%.

[0050] Example 4 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as Example 1, except that the eutectic solvent is choline chloride-benzoic acid.

[0051] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-benzoic acid for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 90%.

[0052] Example 5 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as Example 1, except that the solid-liquid ratio is 5 g L -1 .

[0053] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 80%.

[0054] Example 6 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as Example 1, except that the solid-liquid ratio is 10 g L -1 .

[0055] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 70%.

[0056] Example 7 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as in Example 1, except that the ball milling speed is 200 rpm.

[0057] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co, and Ni can reach more than 30%. Since the mechanical energy is weak at a speed of 200 rpm, the ball milling time is extended to 240 minutes in this embodiment, and the leaching efficiency of Li, Mn, Co, and Ni can reach more than 50%.

[0058] Example 8 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The same scheme as in Example 1, except that the ball milling speed is 400 rpm.

[0059] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni can reach more than 60%.

[0060] Comparative Example 1 A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent 1. Experimental methods The solution is the same as that of Example 1, except that the amount of the grinding aid (mesoporous (α-SiO2·H2O)x(Al2O3)y microspheres, (x=0.1-0.9, y=1-x)) added in step S1 is 0 mg.

[0061] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni is only 40%.

[0062] Comparative Example 2 A method for recovering metal elements from waste ternary lithium batteries by thermochemically driven eutectic solvent 1. Experimental methods The solution is the same as that of Example 1, except that in step S1, stirring at 80° C. is used instead of mechanical ball milling.

[0063] 2. Experimental results According to the above method of the present invention, under mechanochemical driving, after the positive electrode material is leached in choline chloride-ethylene glycol for 120 minutes, the leaching efficiency of Li, Mn, Co and Ni is only 70%.

[0064] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for recovering metal elements from waste ternary lithium batteries by mechanochemically driven eutectic solvent, characterized in that: The following steps are involved: S1. Leaching: The mixture of the cathode material powder of the waste ternary lithium battery, the eutectic solvent and the grinding aid is ball-milled under the action of a ball-milling medium to obtain a leachate; S2 precipitation: the leachate was subjected to graded precipitation to obtain Ni, Co, Mn hydroxide and Li2CO3; The grinding aid is (α-SiO2·H2O) x ·(Al2O3) y Mesoporous microspheres, where x=0.1-0.9, y=1-x.

2. The method according to claim 1, characterized in that The amount of the grinding aid added in step S1 is 60 mg to 150 mg.

3. The method according to claim 1, characterized in that The solid-liquid ratio of the leaching solution in step S1 is 1.0 g L -1 ~10g L -1 .

4. The method according to claim 1, characterized in that: The rotation speed of the ball mill in step S1 is 200 rpm to 600 rpm.

5. The method according to claim 1, characterized in that The rotation speed of the ball mill in step S1 is 200 rpm to 600 rpm.

6. The method according to claim 1, characterized in that In step S1, the eutectic solvent is selected from at least one of choline chloride-ethylene glycol, choline chloride-urea, choline chloride-malonic acid or choline chloride-benzoic acid.

7. The method according to claim 6, characterized in that The molar ratio of choline chloride to ethylene glycol, the molar ratio of choline chloride to urea, the molar ratio of choline chloride to malonic acid or the molar ratio of choline chloride to benzoic acid is 1:1-3.

8. The method according to claim 1, characterized in that The graded precipitation in step S2 comprises the following steps: S21. Separating the first solution from the leachate, adjusting the pH value of the first solution to a pH of 9 to 12, and separating the hydroxides of Ni, Co, and Mn and a second solution; S22. Adding a soluble carbonate to the second solution to separate Li2CO3.

9. The method according to claim 8, characterized in that The pH adjuster for adjusting the pH value of the first solution in step S21 is selected from at least one of NaOH and KOH; and / or, the soluble carbonate in step S22 is selected from at least one of Na2CO3 and K2CO3.

10. The method according to claim 1, characterized in that The recovery method further comprises the following steps: S3. Calcination: calcining the hydroxides of Ni, Co and Mn at 500-700° C. for 3-6 hours to obtain metal oxides of Ni, Co and Mn.

Citation Information

Cited By

  • Method for recycling metal elements in waste ternary lithium battery