Tangku green glaze and preparation method thereof

By mixing inorganic raw materials and additives, combined with specific firing conditions, the problem of Tianmu glaze lacking blue-colored tones in the existing technology is solved, and the unique color and weather resistance of Tianmu green glaze is realized, which enhances the artistic value of porcelain.

CN118878210AActive Publication Date: 2024-11-01LILING HEXING CERAMICS CO LTD

Patent Information

Application Number
CN202410849597.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-01
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

The lack of blue-blue colored Tianmu glaze in the prior art limits the color and style expression of porcelain art.

Method used

By preparing Tianmu green glaze including inorganic raw materials and additives, mixing hematite and magnetite ratios, combining appropriate amounts of titanium dioxide and phosphorus pentoxide, using specific firing temperature and atmosphere conditions, two types of blue and green are formed by blue and blue are formed by blue and blue are formed by combining appropriate amounts of titanium dioxide and phosphorus pentoxide. Glaze in hue.

Benefits of technology

The Tianmu Qing glaze has clear stripes and moderate density, beautiful and atmospheric appearance, and the weather resistance and water resistance of the glaze are improved through phenyl alkoxysilane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878210A_ABST
    Figure CN118878210A_ABST
Patent Text Reader

Abstract

The invention provides temmoku green glaze and a preparation method thereof, and relates to the technical field of temmoku glaze preparation. The glaze slip of the temmoku glaze comprises an inorganic raw material and an auxiliary agent; the inorganic raw materials comprise the following components in parts by mass: 10 parts of frit, 10 to 18 parts of SiO2, 7 to 14 parts of P2O5, 5 to 9 parts of Li2O, 8 to 13 parts of Al2O3, 3 to 5 parts of TiO2, 2 to 4 parts of hematite and 1 to 3 parts of magnetite; the auxiliary agent is prepared from the following components in parts by mass: 10 parts of polyacrylamide, 10 to 15 parts of sodium tripolyphosphate, 5 to 9 parts of sodium carboxymethyl cellulose and 2 to 5 parts of phenylmethyldiethoxysilane. The method for preparing the temmoku green glaze comprises the following steps: S1, preparing glaze slip; S2, spraying the glaze; and S3, firing in a reducing atmosphere. The temmoku green glaze prepared by the invention is cyan blue or turquoise green, and is beautiful and elegant in appearance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of Tianmu glaze preparation, and specifically relates to a Tianmu green glaze and a preparation method thereof. Background Art

[0002] Traditional Tianmu glaze refers to a special black glaze porcelain glaze color, which is famous for its large and small spots that naturally emerge in the black glaze. This glaze color not only gives porcelain a unique style and color, but its diversity of glaze color and texture also makes it an ideal choice for surface decoration of many crafts and daily necessities such as architecture, sculptures, ornaments, tea bowls, etc.

[0003] Today, there are many types of Tianmu glazes, each with its own unique glaze color and pattern, and thus each has its own unique name. For example, Oil Drop Tianmu is famous for its shimmering silver or bean paste-colored dots and spots on the black or dark brown glaze; Wooden Leaf Tianmu uses a special process to burn leaf patterns on the glaze to show the natural texture of leaves; Tortoiseshell Tianmu glaze presents a texture and color similar to tortoise shells, which is unique; Yellow Tianmu attracts the eye with its yellow glaze effect; Partridge Spot Tianmu glaze has a spot texture similar to partridge feathers, which is unique; Star Cup Tianmu glaze is decorated with spots or textures similar to stars, giving people a sense of mystery; Black Ding Cup is famous for its specific black glaze.

[0004] Although there are many colors and patterns of Tianmu glaze in the prior art, there are few Tianmu glazes with a blue-green tone. The blue-green Tianmu glaze is not only unique in color, but also more majestic and smooth in appearance, adding new colors and styles to the art of porcelain. Summary of the invention

[0005] The Tianmu glaze in the prior art does not have a green glaze surface, so the present invention provides a Tianmu green glaze and a preparation method thereof. The Tianmu green glaze of the present invention has unique color and an elegant appearance.

[0006] The present invention solves the above technical problems through the following technical solutions.

[0007] The present invention provides a Tianmu celadon glaze, wherein the glaze slurry comprises an inorganic raw material and an auxiliary agent;

[0008] In parts by mass, the inorganic raw materials include 10 parts of frit, 10 to 18 parts of SiO2, 7 to 14 parts of P2O5, 5 to 9 parts of Li2O, 8 to 13 parts of Al2O3, 3 to 5 parts of TiO2, 2 to 4 parts of hematite, and 1 to 3 parts of magnetite;

[0009] The frit composition includes 40-50wt% SiO2, 10-12wt% B2O3, 9-12wt% CaO, 8-10wt% Al2O3, 2-3wt% MgO, 5.8-7wt% ZnO, 6-8wt% K2O, and 5-7wt% Na2O;

[0010] In parts by mass, the auxiliary agent includes 10 parts of polyacrylamide (CAS No.: 9003-05-8), 10 to 15 parts of sodium tripolyphosphate (CAS No.: 7758-29-4), 5 to 9 parts of sodium carboxymethyl cellulose (CAS No.: 9004-32-4) and 2 to 5 parts of phenyl alkoxy silane.

[0011] In the present invention, the inorganic raw materials include, by mass, 10 parts of frit, 10 to 14 parts of SiO2, 9 to 12 parts of P2O5, 2.8 to 4.3 parts of Li2O, 8.4 to 9.5 parts of Al2O3, 3.7 to 4.4 parts of TiO2, 3.2 to 4.3 parts of hematite and 2.5 to 3.5 parts of magnetite.

[0012] In the present invention, the addition of Li2O can reduce the thermal expansion coefficient, adjust the thermal expansion coefficient of Tianmu celadon glaze, and avoid glaze defects caused by excessive thermal expansion coefficient.

[0013] In the present invention, the auxiliary agent includes 10 parts of polyacrylamide, 10 to 12 parts of sodium tripolyphosphate, and 5 to 7 parts of sodium carboxymethyl cellulose by weight. Among the auxiliary agents of the present invention, sodium tripolyphosphate helps to improve the uniformity and transparency of the glaze slurry; sodium carboxymethyl cellulose is a good thickener and emulsifier, which can adjust the viscosity of the glaze slurry; the dispersion system formed by polyacrylamide is more stable than that of ordinary surfactants; the above-mentioned phenyl alkoxy silane is an organic silicone with good weather resistance, water resistance, and anti-adhesion properties.

[0014] In the present invention, the composition of the frit is 45.8wt% SiO2, 11.3wt% Al2O3, 9.1wt% CaO, 9.9wt% B2O3, 2.7wt% MgO, 6.8wt% ZnO, 7.3wt% K2O, 6.6wt% Na2O, and the rest are unavoidable impurities.

[0015] In the present invention, the phenylalkoxysilane includes at least one of phenyldiethoxysilane (17872-93-4), phenylmethyldiethoxysilane (CAS No.: 775-56-4), methyldiphenylethoxysilane (1825-59-8), and phenyltrimethoxysilane (2996-92-1); preferably, phenyldiethoxysilane or methyldiphenylethoxysilane.

[0016] In the present invention, the mass ratio of the inorganic raw material to the auxiliary agent is 10:1-3, preferably 10:2-2.7.

[0017] In the present invention, the mass ratio of hematite to magnetite is 1.2 to 1.8, preferably 1.3 to 1.6.

[0018] In the present invention, iron elements can form glazes of various colors under a high-temperature reducing atmosphere, and iron ions and ferrous ions can form complexes with phosphates and silicates. The colors of these complexes depend on the ion valence and the chemical properties of the surrounding environment, such as the concentration of iron ions, the ratio of Fe2+ to Fe3+, and the degree of dispersion of iron ions in the glaze, which will affect the color performance. Under the reducing atmosphere of the present invention, when the iron element exists in the form of Fe2+, it will appear blue; and when the iron element exists in the form of Fe3+, it may appear green or yellow.

[0019] In the present invention, the sum of the mass of magnetite and hematite accounts for 6-9% of the total mass of the inorganic raw materials, preferably 7-8.5%. When the sum of the mass of magnetite and hematite accounts for a larger total mass of the inorganic raw materials, the color of the glaze will be darker.

[0020] In the present invention, the mass of the P2O5 accounts for 13-21% of the total mass of the inorganic raw materials, preferably 16-19.5%.

[0021] In the present invention, P2O5 is added as a flux in the glaze slurry, which can help the inorganic raw materials to dissolve and mix better, thereby forming a more uniform microstructure; in addition, phosphorus pentoxide can promote the crystallization of titanium dioxide, which also helps to improve the whiteness of the glaze.

[0022] In the present invention, the TiO2 accounts for 4-9% of the total mass of the inorganic raw materials, preferably 5-8%. The crystals of titanium silicate precipitated by TiO2 will promote the enrichment of iron, thereby forming the stripes of the Tianmo glaze. When too much TiO2 is added, the stripes will be relatively wide, while when too little TiO2 is added, the stripes will be small and sparse.

[0023] In the present invention, the specific gravity of the glaze slurry is 1.43-1.47 g / cm 3 , preferably 1.45~1.48g / cm 3 .

[0024] In the present invention, the flow coefficient of the glaze slurry is 1.24 to 1.37, preferably 1.26 to 1.33.

[0025] In the present invention, the Mw of the polyacrylamide is between 8 and 10 million.

[0026] In the present invention, the polyacrylamide is a cationic polyimide.

[0027] In the present invention, the viscosity of sodium carboxymethyl cellulose is 1500-2800 mPa·s.

[0028] The present invention also provides a method for preparing Tianmu celadon glaze, comprising the following steps:

[0029] S1. Preparation of glaze slurry:

[0030] Wet-grinding and sieving the inorganic raw materials to obtain a mixture; adding water and an additive to the mixture and mixing to obtain a glaze slurry;

[0031] S2. Spray glaze:

[0032] Spraying glaze slurry onto the surface of the blank and then drying to obtain a semi-finished product;

[0033] S3. Firing:

[0034] a. Preheating stage: Heat the semi-finished product to 490-510℃ and preheat for 30-50min. During the preheating stage, the oxygen content is controlled below 2% and the carbon monoxide content is 2-5%;

[0035] b. Insulation stage: heat to 1200-1220℃ and keep warm for 100-150min. The oxygen content is 0.2-0.5% and the carbon monoxide content is 4-8% during the insulation stage.

[0036] c. Cooling: Cool with the furnace to 250-300℃, and then cool with air to 20-30℃ after opening the kiln door. Cooling has a great influence on the crystal shape and color. If it is directly cooled with water or cooled with air, the final result is a dark yellow glaze, and water cooling or cooling with air will also make the stripes unevenly distributed.

[0037] In S1, during the wet grinding process, the mass ratio of ball stone: inorganic raw material: water is 1:1.5:0.7-0.8, wherein the ball stone is a corundum ceramic ball.

[0038] In S1, the wet grinding speed is 400-500 rpm.

[0039] In S1, the wet grinding time is 4 to 8 hours.

[0040] In S2, the glaze spraying thickness is controlled to be 0.25-0.3 mm. If the glaze spraying thickness is too thick, it will lead to difficulty in restoration and fail to present the blue color, while if the glaze spraying thickness is insufficient, it will affect the flatness of the glaze surface.

[0041] In S2, the distance between the glaze spraying gun and the blank is 200-300 mm.

[0042] In S2, the whiteness of the green billet is ≥80%.

[0043] In S2, the thermal expansion coefficient of the blank is 5.33 to 5.48×10 -6 / ℃.

[0044] In S3, the air and moisture in the kiln can be discharged by heating in the early stage of the preheating stage, and part of the iron oxide can be reduced to ferrous oxide and oxygen. The oxygen content in the kiln needs to be discharged during the preheating stage, which is conducive to the control of the color in the subsequent insulation stage. On the other hand, inorganic raw materials with low melting points can also generate corresponding silicates in a reducing atmosphere, because alkaline oxides such as MgO, K2O and Na2O in inorganic raw materials exist in the form of oxides, which are more compatible with acidic oxides (such as P2O5) in the glaze, and finally lead to poor iron enrichment effect. In addition, preheating can make phenylalkoxysilane fully react with inorganic raw materials, forming an organic film on the surface of the glaze, which increases the stain resistance of the glaze.

[0045] In S3, the heating rates of the preheating stage and the heat preservation stage are independently 12-15°C / min.

[0046] In S3, the oxygen content in the preheating stage is controlled at 1.0-1.8%, and the carbon monoxide content is controlled at 2-4%.

[0047] In S3, the oxygen content in the heat preservation stage is controlled at 0.2-0.3%, and the carbon monoxide content is controlled at 6-8%. Wherein, too high or too low oxygen and carbon monoxide content will affect the performance of the glaze color.

[0048] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0049] Compared with the prior art, the present invention has the following beneficial effects:

[0050] 1. The present invention adjusts the ratio of hematite and magnetite, and the ratio of the sum of the masses of the two to the total mass of inorganic raw materials, so that the stripes of Tianmu celadon glaze are clear and the density is moderate. The addition of an appropriate amount of titanium dioxide can promote the enrichment of iron, which is conducive to the formation of stripes; phosphorus pentoxide can act as a dispersant to avoid large-area local enrichment of cyan blocks. Finally, the Tianmu celadon glaze prepared by the present invention has two tones of cyan blue and cyan green, with clear stripes and a beautiful and atmospheric appearance.

[0051] 2. The process of the present invention involves three steps: glaze slurry preparation, glazing and firing. Strict firing temperature, firing reducing atmosphere and cooling method are selected to make the color of Tianmu celadon glaze more unique. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 Surface diagram of glazes prepared in the examples and comparative examples of the present invention. DETAILED DESCRIPTION

[0053] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.

[0054] GB / T 23460.1-2009 Ceramic glaze performance test method Part 1: High temperature fluidity test melt flow method

[0055] The frit components used in the following examples are shown in Table 1:

[0056] Table 1

[0057]

[0058] The raw material information used in the present invention is shown in Table 2:

[0059] Table 2

[0060] name Manufacturer or model Property parameters Polyacrylamide Wengjiang, Guangdong Cationic, Mw.12 million Sodium Carboxymethyl Cellulose Wengjiang, Guangdong Viscosity 1500~2800mPa·s Hematite Hubei Guangao - magnetite Hebei Zhuofei - <![CDATA[TiO2]]> Anatase -

[0061] The surface whiteness of the blank of the present invention is 90%, and the thermal expansion coefficient of the base glaze on the surface of the blank is 5.37×10 -6 / ℃. The thermal expansion coefficient of the glaze of the present invention needs to be controlled within the range of 4.92 to 5.23×10 -6 / ℃, if the difference in thermal expansion coefficients between the blank and the glaze is large, it will cause cracks or even peeling of the glaze. If the difference in thermal expansion coefficients is too small, the glaze will be subjected to compressive stress during the cooling process, which will also cause defects in the glaze.

[0062] Example 1

[0063] 1. The glaze slurry formula of the Tianmu celadon glaze of this embodiment is as follows:

[0064] Inorganic raw materials: 10 parts of frit, 16.7 parts of SiO2, 10 parts of P2O5, 8.3 parts of Li2O, 8.5 parts of Al2O3, 4.4 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0065] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 3 parts of phenyldiethoxysilane.

[0066] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0067] 2. The preparation method of the Tianmu celadon glaze of this embodiment is as follows:

[0068] S1. Preparation of glaze slurry:

[0069] The inorganic raw materials were wet-milled at 400 rpm for 4 hours and passed through a 200-mesh sieve to obtain a mixture; water and additives were added to the mixture and mixed to obtain a glaze slurry. The flow coefficient of the glaze was 1.26, and the specific gravity of the glaze slurry was 1.46 g / cm 3 ;

[0070] S2. Spray glaze:

[0071] The glaze slurry is sprayed onto the surface of the blank, the spray gun is 300mm away from the blank, the spray thickness is 0.3mm, and then dried to obtain a semi-finished product;

[0072] S3. Firing:

[0073] a. Preheating stage: Heat the semi-finished product to 200℃ at a heating rate of 15℃ / min for 40min. Nitrogen is introduced during the preheating stage, and the oxygen content is adjusted to 1.5% and the carbon monoxide content to 3%;

[0074] b. Insulation stage: heat up to 1200℃ at a heating rate of 15℃ / min and keep warm for 130min. The oxygen content is 0.2% and the carbon monoxide content is 6% during the insulation stage.

[0075] c. Cooling: Cool to 300℃ with the furnace, and then cool to 20℃ with air after opening the kiln door.

[0076] The glaze surface obtained in this embodiment is shown in the attached figure Figure 1 Embodiment 1.

[0077] Example 2

[0078] 1. The glaze slurry formula of the Tianmu celadon glaze of this embodiment is as follows:

[0079] Inorganic raw materials: 10 parts of frit, 14 parts of SiO2, 12.7 parts of P2O5, 7.8 parts of Li2O, 11.4 parts of Al2O3, 3.3 parts of TiO2, 3.3 parts of hematite, 2.1 parts of magnetite;

[0080] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 3 parts of methyl diphenyl ethoxy silane.

[0081] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.2.

[0082] 2. The preparation method of Tianmu green glaze in this embodiment is the same as that in Example 1.

[0083] The flow coefficient of the glaze prepared in this embodiment is 1.28, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0084] The glaze surface obtained in this embodiment is shown in the attached figure Figure 1 Embodiment 2.

[0085] Example 3

[0086] 1. The glaze slurry formula of the Tianmu celadon glaze of this embodiment is as follows:

[0087] Inorganic raw materials: 10 parts of frit, 18 parts of SiO2, 13.6 parts of P2O5, 6.8 parts of Li2O, 11.8 parts of Al2O3, 3.7 parts of TiO2, 2.9 parts of hematite, 2.1 parts of magnetite;

[0088] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 4 parts of phenyldiethoxysilane.

[0089] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0090] 2. The preparation method of Tianmu green glaze in this embodiment is the same as that in Example 1.

[0091] The flow coefficient of the glaze prepared in this embodiment is 1.26, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0092] The glaze surface obtained in this embodiment is shown in the attached figure Figure 1 Embodiment 3.

[0093] Comparative Example 1

[0094] 1. The glaze formula of the Tianmu celadon glaze of this comparative example is as follows:

[0095] Inorganic raw materials: 10 parts of frit, 16.7 parts of SiO2, 9 parts of P2O5, 8.3 parts of Li2O, 8.5 parts of Al2O3, 4.4 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0096] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 3 parts of phenyldiethoxysilane.

[0097] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0098] 2. The preparation method of the Tianmu celadon glaze of this comparative example is the same as that of Example 1, except that S3. the firing method is different. Specifically, the firing process is as follows:

[0099] S3. Firing:

[0100] a. Introduce nitrogen into the kiln, and proceed directly to step b after exhausting the air;

[0101] b. Insulation stage: heat up to 1200℃ at a heating rate of 15℃ / min and keep warm for 200min. The oxygen content is 0.2% and the carbon monoxide content is 3% during the insulation stage.

[0102] c. Cooling: Cool to 300℃ with the furnace, and then cool to 20℃ with air after opening the kiln door.

[0103] The flow coefficient of the glaze prepared in this comparative example is 1.26, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0104] The glaze surface obtained in this comparative example is shown in the attached figure Figure 1 Comparative Example 1.

[0105] Comparative Example 2

[0106] 1. The glaze formula of the Tianmu celadon glaze of this comparative example is as follows:

[0107] Inorganic raw materials: 10 parts of frit, 17 parts of SiO2, 9.8 parts of P2O5, 7 parts of Li2O, 8.3 parts of Al2O3, 4.1 parts of TiO2, 5 parts of hematite, 0.8 parts of magnetite;

[0108] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate and 7 parts of sodium carboxymethyl cellulose.

[0109] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0110] 2. The preparation method of Tianmu green glaze in this comparative example is the same as that in comparative example 2.

[0111] The flow coefficient of the glaze prepared in this comparative example is 1.26, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0112] The glaze surface obtained in this comparative example is shown in the attached figure Figure 1 Comparative Example 2.

[0113] Comparative Example 3

[0114] 1. The glaze slurry formula of the Tianmu celadon glaze of this comparative example is as follows:

[0115] Inorganic raw materials: 10 parts of frit, 16.1 parts of SiO2, 8.7 parts of P2O5, 7.3 parts of Li2O, 8.5 parts of Al2O3, 6 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0116] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 3 parts of methyl diphenyl ethoxy silane.

[0117] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0118] 2. The preparation method of Tianmu green glaze in this comparative example is the same as that in Example 1.

[0119] The flow coefficient of the glaze prepared in this comparative example is 1.26, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0120] The glaze surface obtained in this comparative example is shown in the attached figure Figure 1 Comparative Example 3.

[0121] Comparative Example 4

[0122] 1. The glaze slurry formula of the Tianmu celadon glaze of this comparative example is as follows:

[0123] Inorganic raw materials: 10 parts of frit, 18 parts of SiO2, 4 parts of P2O5, 7.3 parts of Li2O, 8.5 parts of Al2O3, 4.4 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0124] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 3 parts of methyl diphenyl ethoxy silane.

[0125] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0126] 2. The preparation method of Tianmu green glaze in this comparative example is the same as that in Example 1.

[0127] The flow coefficient of the glaze prepared in this comparative example is 1.26, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0128] The glaze surface obtained in this comparative example is shown in the attached figure Figure 1 Comparative Example 4.

[0129] Comparative Example 5

[0130] 1. The glaze slurry formula of the Tianmu celadon glaze of this comparative example is as follows:

[0131] Inorganic raw materials: 10 parts of frit, 18 parts of SiO2, 4 parts of P2O5, 7.3 parts of Li2O, 8.5 parts of Al2O3, 4.4 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0132] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 4 parts of methyl diphenyl ethoxy silane.

[0133] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0134] 2. The preparation method of Tianmu celadon glaze in this comparative example is the same as that in Example 1.

[0135] The flow coefficient of the glaze prepared in this comparative example is 1.26, and the specific gravity of the glaze slurry is 1.45 g / cm 3 .

[0136] The glaze surface obtained in this comparative example is shown in the attached figure Figure 1 Comparative Example 5.

[0137] Comparative Example 6

[0138] 1. The glaze slurry formula of the Tianmu celadon glaze of this comparative example is as follows:

[0139] Inorganic raw materials: 10 parts of frit, 16.7 parts of SiO2, 10 parts of P2O5, 8.3 parts of Li2O, 8.5 parts of Al2O3, 4.4 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0140] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 4 parts of methyl diphenyl ethoxy silane.

[0141] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0142] 2. The preparation method of Tianmu celadon glaze in this embodiment is the same as that in embodiment 1, except that c. the cooling method of S3 is different. Specifically, the cooling step is c. cooling: cooling with furnace air at 20°C.

[0143] The glaze surface obtained in this comparative example is shown in the attached figure Figure 1 Comparative Example 6.

[0144] Comparative Example 7

[0145] 1. The glaze slurry formula of the Tianmu celadon glaze of this comparative example is as follows:

[0146] Inorganic raw materials: 10 parts of frit, 16.7 parts of SiO2, 10 parts of P2O5, 8.3 parts of Li2O, 8.5 parts of Al2O3, 4.4 parts of TiO2, 2.6 parts of hematite, 1.7 parts of magnetite;

[0147] Additives: 10 parts of polyacrylamide, 12 parts of sodium tripolyphosphate, 7 parts of sodium carboxymethyl cellulose and 3 parts of methyl diphenyl ethoxy silane.

[0148] The mass ratio of inorganic raw materials: auxiliary agents is 10:2.5.

[0149] 2. The preparation method of Tianmu celadon glaze in this embodiment is the same as that in embodiment 1, except that c. the cooling method of S3 is different. Specifically, the cooling step is c. cooling: cooling with furnace air at 20°C.

[0150] Effect Example

[0151] The test method for thermal expansion coefficient refers to Part 8 of the test method for ceramic tiles: Determination of linear thermal expansion GB / T3810.8-2016. The test method for sewage resistance refers to Part 14 of the test method for ceramic tiles: Determination of pollution resistance GB / T 3810.14-2016.

[0152] The effects of the glaze slurries and the prepared glaze surfaces of the above embodiments and comparative examples are shown in Table 3:

[0153] Table 3

[0154]

[0155] The Tianmu celadon glaze obtained in Examples 1 and 2 is blue in tone. The addition of TiO2 in Example 1 is relatively large compared with that in Example 2. In Example 1, TiO2 forms more titanium silicate crystals, which helps to enrich iron. Therefore, the stripes in Example 1 are denser than those in Example 2. In Example 3, the mass ratio of hematite to magnetite is low, which affects the Fe 2+ and Fe 3+ ratio, resulting in a green hue.

[0156] Comparative Example 1 does not contain a preheating stage, so oxygen and water are not discharged in time. Because there is no preheating stage to promote the formation of metal silicates by alkali metals, it is not conducive to the phase separation of phosphorus pentoxide, so it finally forms a yellowish cyan color, and presents long stripes with more overlapping parts. In Comparative Example 2, the mass ratio of hematite and magnetite is 6.3:1, and the sum of the mass of hematite and magnetite accounts for 9.3% of the total mass of inorganic raw materials. The high content of iron makes the glaze appear brown and the stripes are darker; in addition, Comparative Example 2 does not modify the glaze with phenylalkoxysilane, so the glaze has poor stain resistance. In Comparative Example 3, TiO2 accounts for 9.9% of the total mass of inorganic raw materials, so that the stripes on the glaze are almost overlapping, and the blue and green are not clear enough. In Comparative Example 4, the mass of P2O5 accounts for 7.1% of the total mass of inorganic raw materials. As a dispersed phase, the amount of P2O5 is too small, which will cause the blue-cyan color blocks to be locally enriched, making it difficult to form stripes. In comparative example 5, too little Li2O was added, resulting in a high thermal expansion coefficient of the glaze, which eventually resulted in an uneven glaze surface with glaze defects. In comparative example 6, dark yellow spots were formed with air cooling, and the spots were unevenly distributed.

[0157] Unless otherwise defined, all professional terms used in this article have the same meaning as those generally understood by those skilled in the art. The professional terms used in this article are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or can be prepared by existing methods. The specific embodiments described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A kind of Tianmu celadon glaze, It is characterized in that The glaze slurry includes inorganic raw materials and additives; The inorganic raw materials include 10 parts of frit, 10 to 18 parts of SiO 2 , 7 to 14 portions 2 O 5 , 5~9 parts Li 2 O, 8 to 13 parts of Al 2 O 3 , 3-5 parts TiO 2 , 2 to 4 parts of hematite, 1 to 3 parts of magnetite; The frit composition includes 40-50wt% SiO 2 、10~12wt%B 2 O 3 , 9~12wt%CaO, 8~10wt%Al 2 O 3 , 2~3wt%MgO, 5.8~7wt%ZnO, 6~8wt%K 2 O, 5-7 wt% Na 2 O; In parts by mass, the auxiliary agent includes 10 parts of polyacrylamide, 10 to 15 parts of sodium tripolyphosphate, 5 to 9 parts of sodium carboxymethyl cellulose and 2 to 5 parts of phenylmethyldiethoxysilane.

2. The Tianmu celadon glaze according to claim 1, It is characterized in that The glaze slurry satisfies at least one of the following conditions (1) to (4): (1) In parts by mass, the inorganic raw material includes 10 parts of frit, 10 to 14 parts of SiO 2 , 9 to 12 portions 2 O 5 , 2.8~4.3 parts Li 2 O, 8.4 to 9.5 parts of Al 2 O 3 , 3.7-4.4 parts TiO 2 , 3.2-4.3 parts of hematite and 2.5-3.5 parts of magnetite; (2) The auxiliary agent comprises, by weight, 10 parts of polyacrylamide, 10 to 12 parts of sodium tripolyphosphate, and 5 to 7 parts of sodium carboxymethyl cellulose; (3) The frit composition is 45.8wt% SiO 2 、11.3wt%Al 2 O 3 、9.1wt%CaO、9.9wt%B 2 O 3 , 2.7wt%MgO, 6.8wt%ZnO, 7.3wt%K 2 O, 6.6wt%Na 2 O, the rest are unavoidable impurities; (4) The phenylalkoxysilane includes at least one of phenyldiethoxysilane, phenylmethyldiethoxysilane, methyldiphenylethoxysilane and phenyltrimethoxysilane.

3. The Tianmu celadon glaze according to claim 1, It is characterized in that The mass ratio of the inorganic raw material to the auxiliary agent is 10:1-3, preferably 10:2-2.

7.

4. The Tianmu celadon glaze according to claim 1, It is characterized in that The inorganic raw material satisfies at least one of the following conditions (1) to (4): (1) The mass ratio of hematite to magnetite is 1.2 to 1.8, preferably 1.3 to 1.6; (2) The sum of the mass of magnetite and hematite accounts for 6-9% of the total mass of the inorganic raw materials, preferably 7-8.5%; (3) P 2 O 5 The mass of the inorganic raw materials accounts for 13-21% of the total mass, preferably 16-19.5%; (4) The TiO 2 It accounts for 4-9% of the total mass of the inorganic raw materials, preferably 5-8%.

5. The Tianmu celadon glaze according to claim 1, It is characterized in that The glaze slurry satisfies at least one of the following conditions (1) to (2): (1) The specific gravity of the glaze slurry is 1.43-1.47 g / cm 3 , preferably 1.45~1.48g / cm 3 ; (2) The flow coefficient of the glaze slurry is 1.24 to 1.37, preferably 1.26 to 1.

33.

6. The Tianmu celadon glaze according to claim 1, It is characterized in that The auxiliary agent satisfies at least one of the following conditions (1) to (3): (1) The Mw of the polyacrylamide is between 8 and 12 million; (2) The polyacrylamide is a cationic polyimide; (3) The viscosity of sodium carboxymethyl cellulose is 1500-2800 mPa·s.

7. The method for preparing Tianmu celadon glaze according to claims 1 to 6, It is characterized in that The following steps are involved: S1. Preparation of glaze slurry: Wet-grinding and sieving the inorganic raw materials to obtain a mixture; adding water and an additive to the mixture and mixing to obtain a glaze slurry; S2. Spray glaze: Spraying glaze slurry onto the surface of the blank and then drying to obtain a semi-finished product; S3. Firing: a. Preheating stage: Heat the semi-finished product to 490-510℃ and preheat for 30-50min. During the preheating stage, the oxygen content is controlled below 2% and the carbon monoxide content is 2-5%; b. Insulation stage: heat to 1200-1220℃ and keep warm for 100-150min. The oxygen content is 0.2-0.5% and the carbon monoxide content is 4-8% during the insulation stage. c. Cooling: Cool to 250-300℃ with the furnace, and then cool to 20-30℃ with air after opening the kiln door.

8. The method for preparing Tianmu celadon glaze according to claim 7, It is characterized in that The process for preparing the glaze slurry satisfies at least one of the following conditions (1) to (4): (1) During the wet grinding process, the mass ratio of ball stone: inorganic raw material: water is 1:1.5:0.7-0.8; (2) The wet grinding speed is 400-500 rpm; (3) The wet grinding time is 4 to 8 hours; (4) The mesh size of the sieving is 200 to 250 meshes.

9. The method for preparing Tianmu celadon glaze according to claim 7, It is characterized in that The glaze spraying process satisfies at least one of the following conditions (1) to (4): (1) The glaze spraying thickness is controlled at 0.25-0.3 mm; (2) The distance between the glaze spraying gun and the blank is 200-300 mm; (3) The whiteness of the green billet is ≥80%; (4) The thermal expansion coefficient of the blank is between 5.33 and 5.48 × 10 -6 / ℃.

10. The method for preparing Tianmu celadon glaze according to claim 7, It is characterized in that The firing process satisfies at least one of the following conditions (1) to (3): (1) The heating rates in the preheating stage and the heat preservation stage are independently 12-15°C / min; (2) During the preheating stage, the oxygen content is controlled at 1.0-1.8% and the carbon monoxide content is controlled at 2-4%; (3) During the insulation stage, the oxygen content is controlled at 0.2-0.3% and the carbon monoxide content is controlled at 6-8%.

Citation Information

Patent Citations

  • Preparation process of greyness temmoku oil-spot glaze porcelain

    CN104987045A

  • Colorful pearl glaze material and method for preparing colorful pearl glaze

    CN108892381A

  • Preparation process of crackle-free powder bluish-green glaze craft porcelain

    CN111592344A

  • Jun porcelain celeste blue glazed porcelain and preparation method thereof

    CN112174532A

  • Preparation process of high-strength celeste blue glaze porcelain

    CN113185123A

Cited By

  • Green glaze ceramic chip for analyzing atmosphere in kiln as well as preparation method and application of green glaze ceramic chip

    CN122403770A