Silver sand dry granular glaze and ceramic tile imitating automobile metal paint effect
Through the combination of mica iron oxide, basic glaze and dry particles, combined with color developer, the problem of realizing the automotive metal paint surface effect in ceramics is solved, and the advanced silver flashing effect and silver sand effect of various colors is obtained, which reduces the Cost and simplify the process.
Patent Information
- Application Number
- CN202411374962.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-30
AI Technical Summary
It is difficult for the prior art to achieve the automotive metal paint effect in ceramics, and the existing starlight effect and metal paint effect have problems of high cost and difference in effect.
A combination of mica iron oxide, basic glaze and basic dry particles is used to prepare silver sand dry particles through a specific mass ratio and process flow, and combined with color developer to obtain ceramic tiles that imitate the automotive metal paint effect.
It realizes the advanced decorative effect of silver flashing on the ceramic surface, which is low in cost and simple in process. It can obtain silver sand effect in various colors by adjusting the formula and color developer.
Smart Images

Figure CN118878212B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ceramics, and in particular relates to a silver sand dry particle glaze and a ceramic tile imitating the metal paint surface effect of an automobile. Background Art
[0002] Car metallic paint is also called car metallic flash paint. Tiny metal particles such as aluminum and copper are added to the paint base. When light hits the metal particles, it is reflected through the air film and looks like metal. However, simply applying car paint technology to the ceramic field is obviously not very suitable. The cost is high and the production process is complicated and difficult to repair. The high-temperature treatment during the ceramic firing process will melt the metal particles and react with glaze, dry particles and other materials, losing their own effects and causing many defects on the ceramic glaze. In addition, if this metal material is not handled properly, it will oxidize, making the product unsightly and unstable in quality.
[0003] Among natural stones, there is a kind of granite with dense structure, hard texture, acid and alkali resistance, good weather resistance, and can be used outdoors for a long time. Under the sunlight, golden and dazzling flashes flash through the black and shiny stone surface. This is the precious imported granite that people often call black gold sand. Black gold sand is mainly composed of orthopyroxene and basic plagioclase, containing a small amount of olivine, magnetite and other components. The golden and dazzling gold sand is bronzite. Some manufacturers on the market have imitated the effect of black gold sand granite and developed black gold sand glaze and black gold sand polished glaze, but the effect is inevitably single and the luster is weaker than that of the original stone.
[0004] CN118373708A discloses a glaze and ceramic tile with a starlight effect after firing. The glaze with a starlight effect after firing comprises a base glaze and starlight particles that can present a starlight effect under the irradiation of a light source after firing. The starlight particles are added to the base glaze in an external manner, and the two are mixed evenly to obtain a glaze with a starlight effect after firing. The starlight particles are frit particles obtained by melting, water quenching, crushing and screening the raw materials, and the mass of the starlight particles accounts for ≥2.5% of the mass of the base glaze. The starlight particles are obtained by roller crushing with a roller machine, and the silicon-aluminum ratio in the chemical composition is higher than that of general starlight particles, which is matched with the specific particle size distribution of the starlight particles and the added mass ratio of the starlight particles, so that the starlight particles do not protrude from the surface. After firing, the starlight particles are evenly embedded under the glaze surface, and no polishing is required after firing. Under the light source, the light enters the corners of the starlight particles under the glaze surface, and the reflection obtains a point-like starlight effect similar to stars, thereby obtaining a better glaze surface flatness and pollution resistance. This technology has high requirements for roller crushing and high production costs, and there is also a big difference between its starlight effect and metallic paint effect.
[0005] How to combine car paint silver powder with black gold sand effect to obtain silver sand effect so that ceramics have car metal paint effect is a problem to be solved. Summary of the invention
[0006] The object of the present invention is to overcome at least one disadvantage of the prior art and to provide a silver sand dry granular glaze and ceramic tile with an imitation automobile metal paint effect.
[0007] The technical solution adopted by the present invention is:
[0008] The first aspect of the present invention provides:
[0009] A silver sand dry particle glaze imitating the metallic paint effect of an automobile, wherein the solid phase components are composed of mica iron oxide, basic glaze, and basic dry particles, wherein the mass ratio of mica iron oxide, basic glaze, and basic dry particles is (20-73): (0-70): (30-100), wherein:
[0010] The raw materials of the basic glaze are composed by weight: 5 to 24 parts of potassium feldspar, 35 to 57 parts of sodium feldspar, 3 to 10 parts of quartz, 3 to 18 parts of kaolin, 7 to 26 parts of limestone, 2 to 20 parts of wollastonite, 0 to 3 parts of talc, and 3 to 33 parts of iron oxide red;
[0011] The raw materials of the basic dry particles are composed by weight: 39-62 parts of quartz, 5-8 parts of potassium feldspar, 11-33 parts of sodium feldspar, 2-20 parts of dolomite, 3-10 parts of calcined talc, 3-15 parts of aluminum oxide, 1-10 parts of zinc oxide, and 1-10 parts of strontium carbonate;
[0012] The average particle size of the mica iron oxide is 45 to 230 μm.
[0013] In some examples of silver sand dry grain glaze, the chemical mass composition of the basic glaze is: SiO2: 37-70%, Al2O3: 5-20%, K2O: 1-15%, Na2O: 1-17%, Fe2O3: 6-20%, CaO: 8-20%, MgO: 1-10%, TiO2: 0-0.5% and unavoidable impurities.
[0014] In some examples of silver sand dry particle glaze, the chemical mass composition of the basic dry particles is: SiO2: 44-70%, Al2O3: 5-20%, K2O: 1-10%, Na2O: 3-7%, Fe2O3: 0-1%, CaO: 3-11%, MgO: 2-7%, TiO2: 0-0.5%, ZnO: 1-6%, SrO: 1-8% and unavoidable impurities.
[0015] In some examples of silver sand dry particle glaze, the melting temperature for preparing the basic dry particles is 1400-1600°C.
[0016] In some examples of silver sand dry particle glaze, the melting and heat preservation time for preparing the basic dry particles is 1 to 5 hours.
[0017] In some examples of silver sand dry particle glaze, the melting temperature for preparing the basic dry particles is 1400-1600° C., and the heat preservation time is 1-5 h.
[0018] In some examples of silver sand dry particle glaze, the chemical mass composition of the mica iron oxide is: SiO2: 1-10%, Al2O3: 0.1-5%, K2O: 0.1-2%, Na2O: 0-1%, Fe2O3: 80-99%, CaO: 0.1-1%, MgO: 0.1-1%.
[0019] In some examples of silver sand dry particle glaze, the average particle size of the basic dry particles is 45 to 230 μm, preferably 125 to 325 μm.
[0020] In some examples of silver sand dry particle glaze, the average particle size of mica iron oxide is 125-325 μm.
[0021] In some examples of silver sand dry grain glaze, an appropriate amount of developer is also added.
[0022] In some examples of silver sand dry granular glaze, the color developer includes but is not limited to at least one of inorganic ceramic pigments such as iron oxide, cobalt oxide, copper oxide, nickel oxide, tungsten oxide, and manganese oxide.
[0023] In some examples of silver sand dry particle glaze, the developer accounts for 0.5-10% of the dry weight of the silver sand dry particle glaze, preferably 0.5-5%.
[0024] In some examples of silver sand dry granular glaze, the preparation method thereof includes:
[0025] S1) weighing the basic dry granule raw materials according to the proportion, pouring them into a frit furnace, firing at 1400-1600° C. for 1-5 hours, and then crushing and screening to obtain basic dry granules;
[0026] S2) weighing basic glaze raw materials according to the proportion, pouring them into a blender to obtain basic glaze dry powder;
[0027] S3) mixing mica iron oxide, basic glaze dry powder and basic dry particles according to a proportion, adding a debonding agent, a binder and an appropriate amount of water, and ball-milling into a glaze slurry;
[0028] S4) Adding a color developer into the glaze slurry, adjusting the viscosity and specific gravity to obtain a silver sand dry particle glaze.
[0029] In some examples of silver sand dry granular glaze, the silver sand dry granular glaze has a specific gravity of 1.35-1.68 and a viscosity of 40.72-65.18 cP at 25°C.
[0030] In some examples of silver sand dry particle glaze, the overall fineness of the glaze slurry obtained by ball milling is controlled to be 38-180 μm.
[0031] The above features can be combined arbitrarily unless they conflict with each other.
[0032] The second aspect of the present invention provides:
[0033] A ceramic tile imitating the metallic paint effect of an automobile comprises a body, a surface glaze layer, a ceramic ink printing layer and a silver sand dry particle layer, wherein the silver sand dry particle layer is obtained by firing the silver sand dry particle glaze described in the first aspect of the invention.
[0034] In some examples of ceramic tiles, the firing temperature of the ceramic tiles is 1130-1210°C.
[0035] In some examples of tiles, the firing time of the tiles is 30 to 70 minutes.
[0036] In some examples of ceramic tiles, the firing temperature of the ceramic tiles is 1130-1210° C., and the firing time is 30-70 minutes.
[0037] In some examples of tiles, the glaze layer has a thickness of 0.1-0.4 mm.
[0038] In some examples of tiles, the melting temperature of the glaze layer is 1130-1180°C.
[0039] In some examples of ceramic tiles, the preparation process includes but is not limited to the glaze process: inkjet design patterns on the blank or the surface glaze, positioning or applying the silver sand dry granular glaze on the entire surface through spraying or pouring glaze, firing, semi-polishing or unpolishing.
[0040] The beneficial effects of the present invention are:
[0041] In some embodiments of the present invention, the silver sand dry granular glaze that imitates the metallic paint effect of an automobile is used to refract light through the silver sand dry granular glaze to form a silvery glittering effect that resembles an automobile paint effect, thereby providing a new decorative effect for tiles.
[0042] The silver sand dry particle glaze imitating the automobile metal paint effect in some embodiments of the present invention can be fired to have the automobile metal paint effect by adjusting the basic formula and improving the process. The glaze has a shiny and high-end appearance and is easy to use.
[0043] In some embodiments of the present invention, the silver sand dry particle glaze imitating the automobile metal paint effect can obtain silver sand effects of various colors, such as aluminum mercury, Somato blue, deep gray, Cangling green, etc., by adjusting the type and addition amount of the color developer. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1This is a photograph of the tile sample of Example 1.
[0045] Figure 2 This is a photograph of the tile sample of Example 2.
[0046] Figure 3 This is a photograph of the tile sample of Example 3.
[0047] Figure 4 This is a photograph of the tile sample of Example 4.
[0048] Figure 5 This is a photograph of the tile sample of Example 5.
[0049] Figure 6 This is a photograph of the tile sample of Example 6.
[0050] Figure 7 This is a photograph of the tile sample of Example 7.
[0051] Figure 8 This is a photograph of the tile sample of Example 8.
[0052] Fig. 9 This is a photograph of the tile sample of Comparative Example 1.
[0053] Fig.10 This is a photograph of the tile sample of Comparative Example 2.
[0054] Fig.11 This is a photograph of the tile sample of Comparative Example 3.
[0055] Fig.12 This is a photograph of the tile sample of Comparative Example 4.
[0056] Fig.13 This is a photograph of the tile sample of Comparative Example 5.
[0057] Fig.14 This is a photograph of the tile sample of Comparative Example 6.
[0058] Fig.15 This is a photograph of a tile sample obtained by adding 5% by mass of chrome iron black to the silver sand dry granular glaze of Example 1 and then firing it.
[0059] Fig.16 This is a photograph of a tile sample obtained by adding 3% by mass of cobalt blue to the silver sand dry granular glaze of Example 1 and then firing it.
[0060] Fig.17 This is a photograph of a tile sample obtained by adding 3% by mass of cobalt blue and 2% by mass of wrapped red to the silver sand dry particle glaze of Example 1 and then firing it. DETAILED DESCRIPTION
[0061] The first aspect of the present invention provides:
[0062] A silver sand dry particle glaze imitating the metallic paint effect of an automobile, wherein the solid phase components are composed of mica iron oxide, basic glaze, and basic dry particles, wherein the mass ratio of mica iron oxide, basic glaze, and basic dry particles is (20-73): (0-70): (30-100), wherein:
[0063] The raw materials of the basic dry particles are composed by weight: 39-62 parts of quartz, 5-8 parts of potassium feldspar, 11-33 parts of sodium feldspar, 2-20 parts of dolomite, 3-10 parts of calcined talc, 3-15 parts of aluminum oxide, 1-10 parts of zinc oxide, and 1-10 parts of strontium carbonate;
[0064] The average particle size of the mica iron oxide is 45 to 230 μm.
[0065] In the present invention, the main components of the basic dry particles in the silver sand dry particle glaze are silicon dioxide, aluminum oxide, calcium oxide, potassium oxide, etc., and contain a certain amount of zinc oxide and strontium oxide. Among them: calcium oxide is a divalent alkaline earth metal oxide and a network exosome oxide, and its main function is a stabilizer to increase the chemical stability and mechanical strength of the frit dry particles; at high temperatures, calcium oxide can reduce the viscosity of the frit and promote its melting and clarification. Zinc oxide can form oxygen-zinc tetrahedrons and enter the structural network, making the structure more stable and reducing the thermal expansion coefficient of the foundation. Strontium oxide is a network exosome oxide, and its effect on the frit dry particles is between that of calcium oxide and barium oxide.
[0066] In the present invention, the main components of the basic glaze in the silver sand dry granular glaze are silicon dioxide, aluminum oxide, calcium oxide, ferric oxide, etc. Among them, limestone and wollastonite are used as the main source materials of calcium oxide, which can reduce the viscosity of the glaze at high temperature and play a role in coloring and fluxing during the glaze firing process. Adding iron red to introduce ferric oxide can weaken the influence of the glaze formula on mica iron oxide, so that the mica iron oxide can also maintain its silver sand luster in the glaze.
[0067] In the present invention, the basic dry particles in the silver sand dry particle glaze have a relatively long melting time, and can discharge the gas as much as possible during the material melting process, so that the dry particles have fewer defects when used.
[0068] In some examples of silver sand dry particle glaze, the chemical mass composition of the basic dry particles is: SiO2: 44-70%, Al2O3: 5-20%, K2O: 1-10%, Na2O: 3-7%, Fe2O3: 0-1%, CaO: 3-11%, MgO: 2-7%, TiO2: 0-0.5%, ZnO: 1-6%, SrO: 1-8% and unavoidable impurities.
[0069] In some examples of silver sand dry granule glaze, the melting temperature for preparing the basic dry granule is 1400-1600° C. At this temperature, the raw materials can be melted well to form a uniform frit, which is conducive to obtaining high-quality basic dry granules.
[0070] In some examples of silver sand dry particle glaze, the melting and heat preservation time for preparing the basic dry particles is 1 to 5 hours. By controlling the heat preservation time, the raw materials can be fully mixed after melting.
[0071] In some examples of silver sand dry particle glaze, the melting temperature for preparing the basic dry particles is 1400-1600° C., and the heat preservation time is 1-5 h.
[0072] In some examples of silver sand dry particle glaze, the melting temperature of the basic dry particles during firing is as high as 1250-1400° C. In this way, the raw materials of the lower layer are more conducive to the discharge of gas during the melting process, thereby reducing bubble defects.
[0073] In some examples of silver sand dry grain glaze, the chemical mass composition of the basic glaze is: SiO2: 37-70%, Al2O3: 5-20%, K2O: 1-15%, Na2O: 1-17%, Fe2O3: 6-20%, CaO: 8-20%, MgO: 1-10%, TiO2: 0-0.5% and unavoidable impurities.
[0074] In some examples of silver sand dry granular glaze, the chemical mass composition of the mica iron oxide is: SiO2: 1-10%, Al2O3: 0.1-5%, K2O: 0.1-2%, Na2O: 0-1%, Fe2O3: 80-99%, CaO: 0.1-1%, MgO: 0.1-1%. Studies have shown that this specific composition of mica iron oxide can bring better results.
[0075] In some examples of silver sand dry particle glaze, the average particle size of the basic dry particles is 45-230 μm, preferably 125-325 μm. With such a particle size, it can be better mixed with mica iron oxide particles.
[0076] In some examples of silver sand dry granular glaze, the average particle size of mica iron oxide is 125-325 μm. Data show that at this particle size, a better imitation car metal paint effect can be obtained.
[0077] In some examples of silver sand dry granule glaze, a proper amount of color developer is also added. The role of the developer is to provide corresponding colors for the silver sand dry granule glaze to obtain different colors of silver sand effects, such as aluminum mercury, Somato blue, deep gray, Cangling green, etc.
[0078] In some examples of silver sand dry granular glaze, the color developer includes but is not limited to at least one of inorganic ceramic pigments such as iron oxide, cobalt oxide, copper oxide, nickel oxide, tungsten oxide, and manganese oxide.
[0079] In some examples of silver sand dry particle glaze, the developer accounts for 0.5-10% of the dry weight of the silver sand dry particle glaze, preferably 0.5-5%.
[0080] In some examples of silver sand dry granular glaze, the preparation method thereof includes:
[0081] S1) weighing the basic dry granule raw materials according to the proportion, pouring them into a frit furnace, firing at 1400-1600° C. for 1-5 hours, and then crushing and screening to obtain basic dry granules;
[0082] S2) weighing basic glaze raw materials according to the proportion, crushing and mixing them evenly to obtain basic glaze dry powder;
[0083] S3) mixing mica iron oxide, basic glaze and basic dry particles according to a proportion, adding a debonding agent, a binder and an appropriate amount of water, and ball-milling into a glaze slurry;
[0084] S4) Adding a color developer into the glaze slurry, adjusting the viscosity and specific gravity to obtain a silver sand dry particle glaze.
[0085] In some examples of silver sand dry granular glaze, the specific gravity of the glaze is 1.35-1.68, and the viscosity at 25° C. is 40.72-65.18 cP. Such a glaze with such specific gravity and viscosity is more conducive to glazing.
[0086] In some examples of silver sand dry granular glaze, the overall fineness of the glaze slurry obtained by ball milling is controlled to be 38-180 μm. This fineness is more conducive to obtaining a uniform and stable quality glaze layer.
[0087] The above features can be combined arbitrarily unless they conflict with each other.
[0088] The second aspect of the present invention provides:
[0089] A ceramic tile imitating the metallic paint effect of an automobile comprises a body, a surface glaze layer, a ceramic ink printing layer and a silver sand dry particle layer, wherein the silver sand dry particle layer is obtained by firing the silver sand dry particle glaze described in the first aspect of the invention.
[0090] In some examples of ceramic tiles, the firing temperature of the ceramic tiles is 1130-1210°C.
[0091] In some examples of tiles, the firing time of the tiles is 30 to 70 minutes.
[0092] In some examples of ceramic tiles, the firing temperature of the ceramic tiles is 1130-1210° C., and the firing time is 30-70 minutes.
[0093] In some examples of tiles, the glaze layer has a thickness of 0.1-0.4 mm.
[0094] In some examples of tiles, the melting temperature of the glaze layer is 1130-1180°C.
[0095] In some examples of ceramic tiles, the preparation process includes but is not limited to the glaze process: inkjet design patterns on the blank or the surface glaze, positioning or applying the silver sand dry granular glaze on the entire surface through spraying or pouring glaze, firing, semi-polishing or unpolishing.
[0096] The following disclosure provides many different embodiments or examples for implementing different solutions of the present invention.
[0097] In the following examples, unless otherwise specified, the parts are parts by mass and the percentages are all percentages by mass.
[0098] The raw material composition of the basic dry particles of the silver sand dry particle glaze in different examples is shown in Table 1.
[0099] Table 1. Raw material composition of basic dry particles of silver sand dry particle glaze in different examples
[0100]
[0101] Note: The dosage units of raw materials in the table are parts by mass.
[0102] For the sake of comparison, the preparation methods of the basic dry particles of Examples 1 to 5 and Comparative Examples 1 to 4 are unified as follows:
[0103] The raw materials are weighed according to the proportion, poured into a frit furnace, fired at 1400-1600°C for 4 hours, and then crushed and sieved to obtain the basic dry particles with an average particle size of 125-325 μm.
[0104] The preparation methods of the silver sand dry particle glaze slurry of Examples 1 to 5 and Comparative Examples 1 to 4 are unified as follows:
[0105] The chemical mass composition of the mica iron oxide used is SiO2: 1-7%, Al2O3: 0.1-3%, K2O: 0.8-1.4%, Na2O: 0-0.7%, Fe2O3: 85-97%, CaO: 0.1-0.5%, and MgO: 0.1-0.6%.
[0106] Take 30 parts by mass of mica iron oxide, 100 parts by mass of basic dry particles, appropriate amount of debonding agent, appropriate amount of binder, appropriate amount of water, appropriate amount of color developer, and ball mill to control the specific gravity of the glaze slurry to be 1.42-1.45, the viscosity at 25°C to be 52-56 cP, and the overall fineness to be 38-180 μm.
[0107] The basic glaze raw material compositions of the silver sand dry particle glaze in different examples are shown in Table 2, wherein the basic dry particles are selected from the dry particles prepared in Example 1.
[0108] Table 2. Mass fraction composition of basic glaze raw materials and basic dry particles of silver sand dry particle glaze in different examples
[0109]
[0110] The preparation methods of the silver sand dry particle glaze slurry of Examples 6 to 8 and Comparative Examples 5 to 6 are unified as follows:
[0111] The chemical mass composition of the mica iron oxide used is SiO2: 1-7%, Al2O3: 0.1-3%, K2O: 0.8-1.4%, Na2O: 0-0.7%, Fe2O3: 85-97%, CaO: 0.1-0.5%, and MgO: 0.1-0.6%.
[0112] Take 30 parts by mass of mica iron oxide, weigh 100 parts by mass of basic glaze raw materials and basic dry particles according to the ratio in Table 2, add appropriate amount of debonding agent, appropriate amount of binder, appropriate amount of water, appropriate amount of color developer, and ball mill to control the specific gravity of the glaze slurry to be 1.42-1.45, the viscosity at 25°C to be 52-56 cP, and the overall fineness to be 38-180 μm.
[0113] The preparation methods of Examples 1 to 8, Comparative Examples 1 to 6 and colored silver sand effect tiles are unified as follows:
[0114] Process flow: body → surface glaze → inkjet design → wet application of silver sand dry particle glaze slurry → firing, wherein the thickness of the surface glaze layer is 0.3mm, the thickness of the silver sand dry particle glaze is 0.5mm, the firing temperature is 1130-1220℃, and the time is 50min.
[0115] The fired tiles of Examples 1 to 8 and Comparative Examples 1 to 6 are respectively as follows Figures 1 to 14 shown.
[0116] like Fig. 9 As shown, compared with Example 3, the quartz and alumina contents of Comparative Example 1 are greatly increased beyond the range, resulting in a sharp increase in the melting temperature of the dry particles of the frit, the high-temperature molten state is viscous and difficult to discharge, and some raw materials are not cooked.
[0117] like Fig.10 As shown, compared with Example 1, the quartz and aluminum oxide contents of Comparative Example 2 are greatly reduced to less than the range, while the zinc oxide and strontium carbonate contents are greatly increased to exceed the range, resulting in a decrease in the melting temperature of the dry particles of the frit, exposure of silver sand particles during the firing process of the tile, and a rough glaze surface that hurts the hand.
[0118] like Fig.11As shown, compared with Example 1, the dolomite, talc and strontium carbonate contents of Comparative Example 3 are greatly increased beyond the range, and the zinc oxide and aluminum oxide contents are greatly reduced below the range, resulting in a low temperature of the dry particles of the frit and poor color development, and strong corrosion of the developer during the firing process.
[0119] like Fig.12 As shown, compared with Example 2, the contents of quartz, dolomite, zinc oxide and strontium carbonate in Comparative Example 4 are greatly increased beyond the range, resulting in a low temperature of the frit dry particles but a large melt viscosity, a large amount of gas is generated during the firing process and it is difficult to discharge, affecting the inkjet design and dry particle distribution.
[0120] like Fig.13 As shown, compared with Example 6, Comparative Example 5 did not add iron red, resulting in a weakening of the gloss of part of the mica iron oxide silver sand.
[0121] like Fig.14 As shown, compared with Example 6, the quartz and kaolin contents of Comparative Example 6 are greatly increased beyond the range, while the albite content is reduced to less than the range, resulting in a slightly higher glaze temperature and fogging, affecting the dry granulation effect.
[0122] Preparation of colored silver sand effect tiles:
[0123] like Fig.15 As shown, by adding 5% by mass of chromium iron black to the silver sand dry particle glaze of Example 1, uniformly mixing and firing, a deep gray silver sand effect is obtained.
[0124] like Fig.16 As shown, by adding 3% by mass of cobalt blue to the silver sand dry particle glaze of Example 1, uniformly mixing and firing, a Somato blue silver sand effect is obtained.
[0125] like Fig.17 As shown, by adding 3% by mass of cobalt blue and 2% by mass of wrapped red to the silver sand dry particle glaze of Example 1, uniformly mixing and firing, a lightning purple silver sand effect is obtained.
[0126] The above is a further detailed description of the present invention, which should not be regarded as a limitation on the specific implementation of the present invention. For ordinary technicians in the technical field to which the present invention belongs, simple deduction or replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A silver sand dry granular glaze that imitates the metallic paint effect of a car. It is characterized in that The solid phase components are composed of mica iron oxide, basic glaze and basic dry particles. The mass ratio of mica iron oxide, basic glaze and basic dry particles is (20-73): (0-70): (30-100). The amount of basic glaze is not 0, wherein: The raw materials of the basic glaze are composed by weight: 5 to 24 parts of potassium feldspar, 35 to 57 parts of sodium feldspar, 3 to 10 parts of quartz, 3 to 18 parts of kaolin, 7 to 26 parts of limestone, 2 to 20 parts of wollastonite, 0 to 3 parts of talc, and 3 to 33 parts of iron oxide red; The raw materials of the basic dry particles are composed by weight: 39-62 parts of quartz, 5-8 parts of potassium feldspar, 11-33 parts of sodium feldspar, 2-20 parts of dolomite, 3-10 parts of calcined talc, 3-15 parts of aluminum oxide, 1-10 parts of zinc oxide, and 1-10 parts of strontium carbonate; The average particle size of the mica iron oxide is 45 to 230 μm.
2. The silver sand dry granular glaze according to claim 1, It is characterized in that The chemical composition of the basic glaze is: SiO 2 :37~70%,Al 2 O 3 :5~20%, K 2 O: 1-15%, Na 2 O: 1-17%, Fe 2 O 3 : 6~20%, CaO: 8~20%, MgO: 1~10%, TiO 2 : 0~0.5% and unavoidable impurities.
3. The silver sand dry particle glaze according to claim 1, It is characterized in that The chemical composition of the basic dry particles is: SiO 2 :44~70%,Al 2 O 3 :5~20%, K 2 O: 1-10%, Na 2 O: 3-7%, Fe 2 O 3 : 0~1%, CaO: 3~11%, MgO: 2~7%, TiO 2 : 0~0.5%, ZnO: 1~6%, SrO: 1~8% and unavoidable impurities.
4. The silver sand dry particle glaze according to claim 1, It is characterized in that The melting temperature for preparing the basic dry particles is 1400-1600° C.; and / or the melting holding time for preparing the basic dry particles is 1-5 h.
5. The silver sand dry particle glaze according to claim 1, It is characterized in that The chemical composition of the mica iron oxide is: SiO 2 :1~10%,Al 2 O 3 :0.1~5%, K 2 O: 0.1-2%, Na 2 O: 0-1%, Fe 2 O 3 : 80~97%, CaO: 0.1~1%, MgO: 0.1~1%.
6. The silver sand dry particle glaze according to any one of claims 1 to 5, It is characterized in that The preparation method thereof comprises: Weigh the basic dry granule raw materials according to the proportion, pour them into a frit furnace, burn them at 1400-1600°C for 1-5 hours, and then crush and screen them to obtain basic dry granules; Weigh the basic glaze raw materials according to the proportion, crush and mix them evenly to obtain basic glaze dry powder; Mix mica iron oxide, basic glaze and basic dry particles according to the proportion, add debonding agent, binder and appropriate amount of water, and ball grind into glaze slurry; Add a color developer into the glaze slurry, adjust the viscosity and specific gravity to obtain the silver sand dry particle glaze.
7. The silver sand dry particle glaze according to claim 6, It is characterized in that The specific gravity of the silver sand dry particle glaze is 1.35-1.68, and the viscosity at 25° C. is 40.72-65.18 cP.
8. A tile that imitates the metallic paint effect of a car. It is characterized in that The invention comprises a body, a surface glaze layer, a ceramic ink printing layer and a silver sand dry particle layer, wherein the silver sand dry particle layer is obtained by firing the silver sand dry particle glaze according to any one of claims 1 to 7.
9. The tile according to claim 8, It is characterized in that The firing temperature of the ceramic tile is 1130-1210°C; and / or the firing time is 30-70 minutes.
Citation Information
Patent Citations
Novel sand crystal glaze utilizing mica iron oxide and preparation process of sand crystal glaze
CN104261880A
Wear-resistant ceramic tile with diamond-like luster effect and preparation method of wear-resistant ceramic tile
CN110304945A