Sizing agent for regenerated yarns and preparation method thereof

By preparing a copolymer slurry containing acrylic monomer and styrene, combining sodium montmorillonium and vinyl sulfonic acid, desorption can be achieved without liquid alkali under low temperature conditions, and the regeneration yarn can be solved at high temperatures The strength problems in a strong alkali environment significantly improve the strength performance of the yarn.

CN118878733APending Publication Date: 2024-11-01FUYADA CHEM SUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991867.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The high temperature and strong alkaline environment of the regenerated yarn during the desizing process lead to damage to the fibers, affecting its strength.

Method used

Using slurry prepared by polymerization reaction of acrylic monomers, styrene, ester monomers, carboxylic monomers and amide monomers, combined with sodium montmorillonium and vinyl sulfonic acid, dispersing and initiation through ultrasonic dispersion. The agent reacts to form a copolymer with good water solubility, avoiding high temperature and strong alkali environment, and achieving low temperature deslurry.

Benefits of technology

Desorption is completed at around 80°C, reducing the strength loss of the regenerated yarn and significantly improving the strength performance of the yarn.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959095230000051
    Figure BDA0004959095230000051
  • Figure BDA0004959095230000071
    Figure BDA0004959095230000071
  • Figure BDA0004959095230000081
    Figure BDA0004959095230000081
Patent Text Reader

Abstract

The invention relates to the technical field of textile, and particularly discloses slurry for regenerated yarn and a preparation method of the slurry. The copolymer in the sizing agent has good water solubility in a desizing system, liquid caustic soda and high temperature are not needed during desizing treatment, desizing can be completed at the temperature close to 80 DEG C, and therefore adverse effects of the high temperature and the strong alkaline environment in the desizing process on regenerated yarn are avoided, and the quality of the regenerated yarn is improved. And the regenerated yarn with better strength performance can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of textile technology, and more specifically, to a slurry for regenerated yarn and a preparation method thereof. Background Art

[0002] Sizing refers to a surface treatment technology for yarn or fabric during the textile production process. This process usually involves evenly coating one or more chemical slurries on the surface of the yarn or fabric to give the yarn or fabric certain physical and chemical properties. After sizing and weaving, in order to smoothly carry out the dyeing process, refining and desizing treatment is required. The commonly used auxiliaries in this treatment link are liquid alkali and refining agents. Recycled yarn usually refers to yarn made from waste textile materials through processes such as washing, crushing, melting and respinning. It has the advantages of environmental protection and recyclability. However, due to the limitations of raw materials and production processes, recycled yarn often has disadvantages such as low strength and weak bonding between fibers. Sizing is an important way to improve these properties.

[0003] Related technology There is a textile process in which the sizing material used in the sizing process is a copolymer of four monomers, namely acrylic acid, methyl acrylate, ethyl acrylate and butyl acrylate, which is neutralized with ammonia water. The liquid alkali used in the desizing process is a sodium hydroxide solution, the amount of liquid alkali used is 5g / L, the amount of refining agent used is 2g / L, and the desizing needs to be carried out at a high temperature of 130°C.

[0004] Regarding the above-mentioned related technologies, the inventors believe that although the desizing process in the related technologies can desize the sized yarn, for the regenerated yarn, the high temperature and strong alkaline environment during the desizing process will cause damage to the fibers in the yarn and have a negative impact on the strength of the regenerated yarn. Summary of the invention

[0005] In the related art, the high temperature and strong alkaline environment during the desizing process will have a negative impact on the strength of the regenerated yarn. In order to improve this defect, the present application provides a slurry for regenerated yarn and a preparation method thereof.

[0006] In the first aspect, the present application provides a slurry for regenerated yarn, using the following technical solution: A slurry for regenerated yarn is obtained by polymerization reaction of raw materials containing the following parts by weight: 606-639 parts of acrylic monomers, 52-56 parts of styrene, 5-7 parts of molecular weight regulators, 80-84 parts of ammonia water, and 5-7 parts of initiators; the acrylic monomers include 296-305 parts by weight of ester monomers, 130-144 parts by weight of carboxylic acid monomers, and 180-190 parts by weight of amide monomers.

[0007] By adopting the above technical solution, the present application optimizes the slurry formula system, uses ester monomers, carboxylic acid monomers and amide monomers together as acrylic monomers, and adds styrene as an auxiliary monomer. At the same time, the present application also limits the usage range of ester monomers, carboxylic acid monomers and amide monomers. Through the combination of the above three types of acrylic monomers and styrene, the copolymer in the slurry can have good water solubility. Therefore, during the desizing treatment, there is no need to use liquid alkali and high temperature, and the desizing can be completed at around 80°C, thereby avoiding the negative impact of high temperature and strong alkaline environment on the strength of the regenerated yarn during the desizing process, which helps to obtain regenerated yarn with better strength performance.

[0008] Preferably, the ester monomers include butyl acrylate and isooctyl acrylate, the carboxylic acid monomers include acrylic acid and methacrylic acid, and the amide monomers include acrylamide.

[0009] By adopting the above technical scheme, the present application preferably selects specific types of ester monomers, carboxylic acid monomers and amide monomers. The slurry obtained by polymerizing these monomers can be desized at a relatively low temperature without the aid of liquid alkali, which helps to obtain regenerated yarn with better strength performance.

[0010] Preferably, the acrylic monomer comprises the following components in parts by weight: 196-200 parts of butyl acrylate, 100-105 parts of isooctyl acrylate, 50-60 parts of acrylic acid, 80-84 parts of methacrylic acid, and 180-190 parts of acrylamide.

[0011] By adopting the above technical scheme, the present application further optimizes the dosage range of each monomer. After the monomers selected according to the above dosage range undergo polymerization reaction, the obtained slurry can be desized at a relatively low temperature without the aid of liquid alkali, which helps to obtain regenerated yarn with better strength performance.

[0012] In a second aspect, the present application provides a method for preparing a slurry for regenerated yarn, using the following technical solution.

[0013] A method for preparing a slurry for regenerated yarn comprises the following steps: (1) adding water to a reaction container, then adding an acrylic monomer, styrene and a molecular weight regulator into the reaction container, and obtaining a monomer dispersion after ultrasonic dispersion for standby use; (2) adding an initiator into a reaction container and stirring the reaction under heating conditions; after the addition of the initiator, adjusting the temperature and keeping the reaction warm for a period of time; and then adding ammonia water into the reaction container for neutralization to obtain a slurry for the regenerated yarn.

[0014] By adopting the above technical solution, the present application first disperses the acrylic monomer, styrene and molecular weight regulator by ultrasonic dispersion to obtain a monomer dispersion with relatively uniform monomer distribution, and then adds an initiator to react. After the reaction is completed, ammonia water is used for neutralization to obtain a slurry for regenerated yarn. The slurry prepared according to the above method can be desized without the aid of liquid alkali and high temperature, which can reduce the strength loss of the regenerated yarn and help to obtain a regenerated yarn with better strength performance.

[0015] Preferably, in step (1) of the preparation method, a slurry modifier, an acrylic monomer, styrene and a molecular weight regulator are added together into a reaction container, and the components of the slurry modifier include sodium montmorillonite and water.

[0016] By adopting the above technical solution, sodium montmorillonite has a natural layered structure, and the copolymer chain segments of acrylic monomers can be intercalated into these layers to form intercalated composites. The formation of intercalated composites can improve the adhesion of the slurry to the yarn, and sodium montmorillonite can reinforce the copolymer through its own mechanical properties, so the addition of sodium montmorillonite can improve the strength performance of the regenerated yarn.

[0017] Preferably, the raw material components of the slurry also include vinyl sulfonic acid.

[0018] By adopting the above technical solution, vinyl sulfonic acid can form a copolymer with acrylic monomer under the action of an initiator, and introduce sulfonic acid groups into the copolymer, which are further converted into anionic groups after being neutralized with ammonia water. This anionic group has a strong electrostatic adsorption effect with the particles of sodium montmorillonite, which can promote the formation of intercalation complexes and help improve the strength performance of the regenerated yarn.

[0019] Preferably, the weight ratio of the vinyl sulfonic acid to the sodium montmorillonite in the slurry modifier is 1:(20-25).

[0020] By adopting the above technical solution, the present application optimizes the weight ratio of vinyl sulfonic acid to sodium montmorillonite, which helps to improve the strength performance of the regenerated yarn.

[0021] Preferably, the slurry further comprises modified nanotubes, and the modified nanotubes are prepared by the following method: (1) adding halloysite nanotubes into water for ultrasonic dispersion to obtain a first dispersion, and mixing the first dispersion with anhydrous ethanol to obtain a second dispersion; (2) Adding a terminal vinyl silane coupling agent to the second dispersion, continuing to stir the reaction, washing, filtering, drying and grinding to obtain modified nanotubes.

[0022] By adopting the above technical solution, the present application uses a terminal vinyl silane coupling agent to modify the halloysite nanotubes to obtain modified nanotubes with vinyl groups on the surface. Under the action of the initiator, the modified nanotubes can participate in the copolymerization reaction of acrylic monomers through the vinyl groups on the surface, thereby using the mechanical properties of the halloysite nanotubes to reinforce the acrylic copolymer, which helps to improve the strength of the regenerated yarn.

[0023] Preferably, the raw material components of the slurry also include vinyl silicone oil.

[0024] By adopting the above technical solution, under the action of the initiator, the vinyl silicone oil can participate in the copolymerization reaction of the acrylic monomer and introduce the organic silicon segment into the formed copolymer. The organic silicon segment has good flexibility, which can make the slurry more fully cover the regenerated yarn, which helps to improve the strength performance of the regenerated yarn.

[0025] Preferably, the weight ratio of the vinyl silicone oil to the initiator is (10-20):1.

[0026] By adopting the above technical solution, the present application optimizes the weight ratio of vinyl silicone oil to initiator, which helps to improve the strength of the regenerated yarn.

[0027] In summary, this application has the following beneficial effects: 1. The copolymer in the slurry of the present application has good water solubility in the desizing system. During the desizing treatment, there is no need to use liquid alkali and high temperature, but the desizing can be completed at around 80°C, thereby avoiding the influence of high temperature and strong alkaline environment during the desizing process on the regenerated yarn, which is helpful to obtain regenerated yarn with better strength performance.

[0028] 2. In the method of the present application, a slurry modifier containing sodium montmorillonite is used, and the adhesion effect of the slurry on the yarn is enhanced by the intercalation effect between the chain segments of the acrylic copolymer and the sodium montmorillonite. The mechanical properties of the sodium montmorillonite are used to reinforce the copolymer, thereby improving the strength performance of the regenerated yarn.

[0029] 3. The present application also adds vinyl silicone oil to the raw material components of the slurry. The silicone chain segments introduced by the vinyl silicone oil have good flexibility, thereby increasing the sizing rate of the slurry, allowing the slurry to more fully coat the regenerated yarn, and helping to improve the strength performance of the regenerated yarn. DETAILED DESCRIPTION

[0030] The present application is further described in detail below in conjunction with embodiments, preparation examples and comparative examples. The raw materials involved in the present application can all be obtained commercially.

[0031] Preparation example of modified nanotubes The following is an explanation using Preparation Example 1.

[0032] Preparation Example 1 In this preparation example, the modified nanotubes were prepared according to the following method: (1) adding 2 kg of halloysite nanotubes to 30 L of water for ultrasonic dispersion to obtain a first dispersion, and mixing the first dispersion with 30 L of anhydrous ethanol to obtain a second dispersion; (2) Add 0.5 kg of vinyltriethoxysilane to the second dispersion, continue stirring at a rate of 200 r / min for 10 h, then wash, filter, dry and grind to obtain modified nanotubes. Example

[0033] Examples 1-5 The following description is given by taking Example 1 as an example.

[0034] Example 1 This embodiment provides a slurry for regenerated yarn, which is obtained by polymerization reaction of the following raw materials in parts by weight: 606 kg of acrylic monomer, 52 kg of styrene, 5 kg of molecular weight regulator, 80 kg of ammonia water (in terms of monohydrated ammonia), and 5 kg of initiator; the acrylic monomer includes 296 kg of ester monomer, 130 kg of carboxylic acid monomer, and 180 kg of amide monomer; the ester monomer is 196 kg of butyl acrylate and 100 kg of isooctyl acrylate, the carboxylic acid monomer is 50 kg of acrylic acid and 80 kg of methacrylic acid, and the amide monomer is 180 kg of acrylamide. The molecular weight regulator is α-methylstyrene dimer, and the initiator is BPO.

[0035] This embodiment provides a method for preparing a slurry for regenerated yarn, comprising the following steps: (1) Add 1200 kg of water to a reaction container, then add acrylic monomer, styrene and molecular weight regulator according to the formula amount into the reaction container, and ultrasonically disperse at a power of 500 W for 30 minutes to obtain a monomer dispersion liquid for standby use; (2) The initiator is added into a reaction vessel and stirred at 40 r / min under heating conditions of 82°C. After the addition of the initiator, the temperature is adjusted to 90°C and kept for reaction for 3 hours. Then the temperature is lowered to 45°C, the stirring rate is quickly increased to 60 r / min, and then ammonia water is added to the reaction vessel for neutralization to obtain a slurry for the regenerated yarn.

[0036] As shown in Table 1, the main difference between Examples 1-5 is that the raw material ratios of the slurry are different.

[0037] Table 1 Ratio of raw materials for slurry Example 6 The difference between this embodiment and embodiment 5 is that in step (1) of preparing the slurry, the slurry modifier, acrylic monomer, styrene and molecular weight regulator are put into the reaction container together, and the component of the slurry modifier is a mixture of sodium montmorillonite and water in a weight ratio of 1:2, and the weight of the sodium montmorillonite is 3.5% of the total weight of the slurry raw materials.

[0038] Example 7 The difference between this embodiment and embodiment 6 is that the raw material components of the slurry also include vinyl sulfonic acid, the weight ratio of vinyl sulfonic acid to sodium montmorillonite in the slurry modifier is 1:30, and the timing of adding vinyl sulfonic acid is the same as that of the acrylic monomer.

[0039] Example 8 The difference between this embodiment and embodiment 7 is that the weight ratio of vinyl sulfonic acid to sodium montmorillonite in the slurry modifier is 1:25.

[0040] Example 9 The difference between this embodiment and embodiment 7 is that the weight ratio of vinyl sulfonic acid to sodium montmorillonite in the slurry modifier is 1:22.

[0041] Example 10 The difference between this embodiment and embodiment 7 is that the weight ratio of vinyl sulfonic acid to sodium montmorillonite in the slurry modifier is 1:20.

[0042] Embodiment 11 The difference between this embodiment and embodiment 10 is that the components of the slurry also include modified nanotubes. The modified nanotubes are prepared according to the method of preparation example 1. The amount of the modified nanotubes is 1% of the total weight of the acrylic acid monomers. The timing of adding the modified nanotubes is the same as that of the acrylic acid monomers.

[0043] Example 12 The difference between this embodiment and embodiment 11 is that the raw material components of the slurry also include vinyl silicone oil, and the weight ratio of vinyl silicone oil to initiator is 8: 1. The vinyl silicone oil is a mixture of branched vinyl silicone oil and terminal vinyl silicone oil in a weight ratio of 1: 3, the model of the branched vinyl silicone oil is IOTA-272, and the model of the terminal vinyl silicone oil is RH-Vi500E.

[0044] As shown in Table 2, the difference between Examples 12-16 is that the weight ratio of vinyl silicone oil to initiator is different.

[0045] Table 2 Weight ratio of vinyl silicone oil and initiator sample Weight ratio of vinyl silicone oil and initiator Example 12 8:1 Example 13 10:1 Embodiment 14 13:1 Embodiment 15 17:1 Example 16 20:1 Embodiment 17 The difference between this embodiment and embodiment 1 is that all acrylic acid is replaced by methacrylic acid.

[0046] Embodiment 18 The difference between this embodiment and embodiment 1 is that all methacrylic acid is replaced by acrylic acid.

[0047] Embodiment 19 The difference between this embodiment and embodiment 1 is that all butyl acrylate is replaced by isooctyl acrylate.

[0048] Embodiment 20 The difference between this embodiment and embodiment 1 is that all isooctyl acrylate is replaced by butyl acrylate.

[0049] Comparative Example Comparative Example 1 The comparative example provides a textile pulp, which is obtained by polymerization reaction of the following raw materials in parts by weight: 606 kg of acrylic monomer, 5 kg of molecular weight regulator, 80 kg of ammonia water (calculated as monohydrated ammonia), and 5 kg of initiator; the acrylic monomer includes 196 kg of methyl acrylate, 100 kg of isoethyl acrylate, 130 kg of acrylic acid, and 180 kg of butyl acrylate. The molecular weight regulator is α-methylstyrene dimer, and the initiator is BPO.

[0050] This comparative example also provides a method for preparing a textile pulp, comprising the following steps: (1) Add 1200 kg of water to a reaction container, then add an acrylic acid monomer and a molecular weight regulator according to the dosage of the formula into the reaction container, and ultrasonically disperse at a power of 500 W for 30 minutes to obtain a monomer dispersion for standby use; (2) Adding the initiator into the reaction vessel, stirring the reaction at a rate of 40 r / min under heating conditions of 82° C., adjusting the temperature to 90° C. and keeping the temperature for 3 h after the initiator is added, then cooling to 45° C., increasing the stirring rate to 60 r / min, and then adding ammonia water to the reaction vessel for neutralization to obtain a textile pulp.

[0051] Comparative Example 2 The difference between this comparative example and Example 1 is that the raw material components of the slurry do not include styrene.

[0052] Comparative Example 3 The difference between this comparative example and Example 1 is that acrylamide is replaced by butyl acrylate of the same weight.

[0053] Comparative Example 4 This comparative example is different from Example 1 in that methacrylic acid is replaced with butyl acrylate in an equal weight.

[0054] Comparative Example 5 The difference between this comparative example and Example 1 is that acrylic acid is replaced by the same weight of butyl acrylate.

[0055] Performance testing methods In the following tests, the regenerated yarn was selected from 50 / 50 regenerated silk protein fiber / cotton fiber blended yarn (147tex / 2, whiteness 67.8%, breaking strength 420cN, breaking elongation 7.5%).

[0056] 1. Desizing rate The specific steps for determining the desizing rate are as follows: (1) Take a certain amount of regenerated yarn, dry it to constant weight, and measure the weight of the regenerated yarn, which is recorded as the weight before sizing (W); (2) The slurry of each embodiment and comparative example was diluted to a slurry with a solid content of 1%, and the regenerated yarn was immersed in the slurry heated to 90° C. After 5 minutes, it was taken out and dried, and then hung in an environment of 20° C. and RH65% for 24 hours and then dried to constant weight. The weight of the regenerated yarn at this time was measured and recorded as the weight after sizing (W1); (3) Immerse the regenerated yarn in the desizing system, take it out after 20 minutes, wash it with 80°C hot water and 15°C cold water, and then dry it to constant weight. Measure the weight of the regenerated yarn at this time and record it as the weight after desizing (W2); (4) Repeat step (3) using the regenerated yarn that has not been sizing treated (weight is denoted as W0), and then measure the weight of the regenerated yarn, which is denoted as W0'.

[0057] After measuring the above parameters, the hairiness loss rate β is calculated according to the following formula: Then calculate the sizing rate S according to the following formula: Then calculate the yarn size content S' after desizing according to the following formula: Finally, the desizing rate S0 is calculated according to the following formula: The test results of desizing rate S0 are shown in Table 3.

[0058] In the above test, comparative example 1 is divided into an experimental group and a control group. The desizing system process parameters corresponding to the slurry of the experimental group are: heating temperature 130°C, sodium hydroxide dosage 5g / L, refining agent dosage 2g / L, and refining agent Superstain XC. The desizing system process parameters corresponding to the control group, comparative examples 2-5, and embodiments 1-20 are: heating temperature 80°C, refining agent dosage 2g / L, and refining agent Superstain XC.

[0059] 2. Relative Strength With reference to the record of GB / T 3916-2013 Determination of breaking strength and breaking elongation of single yarn of textile packaged yarn (CRE method) , the breaking strength of the regenerated yarn after the desizing rate test was tested, and the breaking strength of comparative example 1 was used as a benchmark to calculate the ratio between the breaking strength of each embodiment and comparative example and the breaking strength of comparative example 1, and the ratio was recorded as relative strength. The results are shown in Table 3.

[0060] Table 3 Test results Combining the test group and the control group of Comparative Example 1 and Table 3, it can be seen that the desizing rate of the test group is above 90%, while the desizing rate of the control group is lower, indicating that the sizing material of Comparative Example 1 needs to be fully desized in a high temperature and strong alkaline environment. According to the relative strength test results, it can be seen that the desizing operation adopted by the test group of Comparative Example 1 has a significant negative impact on the breaking strength of the regenerated yarn.

[0061] Combining Examples 1-5 and Comparative Example 1 and Table 3, it can be seen that the desizing rates measured in Examples 1-5 are close to that of the test group of Comparative Example 1, while the relative strength is close to that of the control group of Comparative Example 1, indicating that the sizing agent of the present application achieves a more thorough desizing at a lower temperature, and because the desizing temperature is low, the negative impact on the breaking strength of the regenerated yarn is relatively small.

[0062] Combining Example 1 and Comparative Examples 2-5 and Table 3, it can be seen that the desizing rate of Example 1 is much higher than that of Comparative Examples 2-5, while the relative strength is close to that of Comparative Examples 2-5, indicating that when the raw material components of the slurry do not include styrene, or when the amount of the ester monomer, carboxylic acid monomer, and amide monomer in the acrylic monomer does not meet the range specified in the present application, the desizing effect of the slurry is poor.

[0063] Combining Example 5 and Example 6 with Table 3, it can be seen that the relative strength measured in Example 6 is higher than that in Example 5, indicating that the addition of sodium-based montmorillonite makes the slurry have a more significant effect on improving the strength of the regenerated yarn.

[0064] Combining Example 6 and Example 7 with Table 3, it can be seen that the relative strength measured in Example 7 is higher than that in Example 6, indicating that the addition of vinyl sulfonic acid makes the slurry have a more significant effect of improving the strength of the regenerated yarn.

[0065] Combining Examples 7-10 and Table 3, it can be seen that when the weight ratio of vinyl sulfonic acid to sodium montmorillonite in the slurry modifier is 1:(20-25), the addition of vinyl sulfonic acid enables the slurry to have a more significant effect on improving the strength of the regenerated yarn.

[0066] Combining Example 10, Example 11 and Table 3, it can be seen that the relative strength measured in Example 11 is higher than that in Example 10, indicating that the addition of modified nanotubes makes the slurry have a more significant effect on improving the strength of the regenerated yarn.

[0067] It can be seen from Example 11, Examples 12-16 and Table 3 that the addition of vinyl silicone oil can make the slurry have a more significant effect on improving the strength of the regenerated yarn. When the weight ratio of vinyl silicone oil to initiator is (10-20):1, this effect is more obvious.

[0068] It can be seen from Example 1, Examples 17-20 and Table 3 that when methacrylic acid and acrylic acid are not used in combination, or when butyl acrylate and isooctyl acrylate are not used in combination, the desizing effect of the slurry is poor.

[0069] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A slurry for recycled yarn, It is characterized in that The invention is obtained by polymerization reaction of the following raw materials in parts by weight: 606-639 parts of acrylic monomers, 52-56 parts of styrene, 5-7 parts of molecular weight regulators, 80-84 parts of ammonia water, and 5-7 parts of initiators; the acrylic monomers include 296-305 parts by weight of ester monomers, 130-144 parts by weight of carboxylic acid monomers, and 180-190 parts by weight of amide monomers.

2. The slurry for regenerated yarn according to claim 1, It is characterized in that The ester monomers include butyl acrylate and isooctyl acrylate, the carboxylic acid monomers include acrylic acid and methacrylic acid, and the amide monomers include acrylamide.

3. The slurry for regenerated yarn according to claim 2, It is characterized in that The acrylic monomer comprises the following components in parts by weight: 196-200 parts of butyl acrylate, 100-105 parts of isooctyl acrylate, 50-60 parts of acrylic acid, 80-84 parts of methacrylic acid, and 180-190 parts of acrylamide.

4. A method for preparing a slurry for regenerated yarn according to any one of claims 1 to 3, It is characterized in that The following steps are involved: (1) Adding water to a reaction container, then adding acrylic monomer, styrene and molecular weight regulator into the reaction container, and obtaining a monomer dispersion after ultrasonic dispersion for standby use; (2) Adding an initiator into a reaction container and stirring the reaction under heating conditions, adjusting the temperature after the addition of the initiator and keeping the temperature for a period of time, and then adding ammonia water to the reaction container for neutralization to obtain a slurry for the regenerated yarn.

5. The method for preparing a slurry for regenerated yarn according to claim 4, It is characterized in that In step (1) of the preparation method, a slurry modifier, an acrylic monomer, styrene and a molecular weight regulator are put into a reaction container together, and the components of the slurry modifier include sodium montmorillonite and water.

6. The method for preparing a slurry for regenerated yarn according to claim 5, It is characterized in that The raw material components of the slurry also include vinyl sulfonic acid.

7. The method for preparing a slurry for regenerated yarn according to claim 6, It is characterized in that The weight ratio of the vinyl sulfonic acid to the sodium montmorillonite in the slurry modifier is 1:(20-25).

8. The method for preparing a slurry for regenerated yarn according to claim 4, It is characterized in that The components of the slurry also include modified nanotubes, and the modified nanotubes are prepared according to the following method: (1) adding halloysite nanotubes into water for ultrasonic dispersion to obtain a first dispersion, and mixing the first dispersion with anhydrous ethanol to obtain a second dispersion; (2) Adding a terminal vinyl silane coupling agent to the second dispersion, continuing to stir the reaction, washing, filtering, drying and grinding to obtain modified nanotubes.

9. The method for preparing a slurry for regenerated yarn according to claim 4, It is characterized in that The raw material components of the slurry also include vinyl silicone oil.

10. The method for preparing a slurry for regenerated yarn according to claim 9, It is characterized in that The weight ratio of the vinyl silicone oil to the initiator is (10-20):1.