Modified diatomite ceramic flame-retardant ethylene propylene diene monomer composite material as well as preparation method and application thereof

Through the combination technology of modified diatomaceous earth and acrylic polymer-coated glass powder, the problem of ethylene propylene rubber flame retardant affecting thermal stability and ceramicization treatment to reduce adhesion is solved, and efficient ceramicization is achieved The flame retardant effect improves the flame retardant performance and safety of the material.

CN118878993AInactive Publication Date: 2024-11-01武汉捷沃汽车零部件有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124516.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The flame retardants of existing EPDM rubber often affect their thermal stability and physical properties, and traditional ceramicization treatment will reduce adhesion and limit their application.

Method used

Modified diatomaceous earth and acrylic polymers are used to coat glass powder, and modified diatomaceous earth is treated by plasma, acid and alkali to increase its active groups and negative charges, stabilize the adsorption of flame retardants, and through acrylic polymerization The substance releases glass powder at high temperatures, forming a ceramicized flame retardant barrier.

Benefits of technology

It significantly improves the flame retardant performance and heat resistance of EPDM composite materials, ensures its safety and flame retardant effect at high temperatures, and is suitable for the development of the EPDM industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878993A_ABST
    Figure CN118878993A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of rubber materials, and relates to a modified diatomite ceramic flame-retardant ethylene propylene diene monomer composite material as well as a preparation method and application thereof. The rubber composite material comprises ethylene propylene diene monomer, zinc oxide, stearic acid, sulfur, tetramethylthiuram disulfide, paraffin oil, montmorillonite, talcum powder, modified diatomite, a flame retardant and modified glass powder. According to the invention, the filler diatomite and the glass powder are modified, so that the obtained ethylene propylene diene monomer composite material has good flame retardant property, and along with the temperature rise of the ethylene propylene diene monomer composite material, the modified diatomite, the modified glass powder, the flame retardant and other fillers in the ethylene propylene diene monomer composite material have a synergistic effect and jointly exert a ceramic flame retardant effect; the safety of the EPDM composite material is greatly improved, and the EPDM composite material is of great significance to the development of the EPDM industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber materials and relates to a modified diatomite ceramic flame-retardant EPDM rubber composite material and a preparation method and application thereof. Background Art

[0002] EPDM is a copolymer of ethylene, propylene and a small amount of non-conjugated dienes. It is a type of ethylene-propylene rubber, represented by EPDM (Ethylene Propylene Diene Monomer). Because its main chain is composed of chemically stable saturated hydrocarbons and only contains unsaturated double bonds in the side chains, it has excellent aging resistance such as ozone resistance, heat resistance, and weather resistance. At the same time, among all rubbers, EPDM has the lowest specific gravity and can absorb a large amount of fillers and oils without much effect on the properties, so it can be made into low-cost rubber compounds. At present, EPDM is widely used in automotive parts, waterproof materials for construction, wire and cable sheaths, heat-resistant hoses, tapes, automotive seals and other fields. However, the EPDM in the prior art is flammable, so it is particularly important to study its flame retardancy.

[0003] At present, the research on EPDM flame retardants has encountered many problems. For example, some flame retardants will affect the thermal stability of EPDM, resulting in a decrease in the heat resistance of the material or a gradual weakening of the flame retardant effect during long-term use; and some flame retardants will have a negative impact on the physical properties of EPDM (such as tensile strength, wear resistance, etc.), which will limit the use of EPDM in specific applications. For example, a Chinese patent application with publication number CN115975297A discloses a method for preparing flame-retardant EPDM rubber. The raw materials and their proportions used in the preparation of the rubber are 100 parts of EPDM rubber; 24 to 26 parts of kaolin; 0.4 to 10.6 parts of antioxidant; 0.6 to 0.9 parts of antioxidant; 17 to 25 parts of flame retardant; 0.6 to 0.8 parts of flow agent; and 1 to 2.5 parts of vulcanizing agent. Decabromodiphenylethane and antimony trioxide are used as flame retardants to achieve the flame retardant effect. However, decabromodiphenylethane (DecaBDE), as a persistent organic pollutant (POPs), is difficult to degrade in the environment, is easy to accumulate and has bioaccumulation, and may cause potential harm to the ecosystem and human health. In addition, some scholars have proposed using thermal spraying or chemical vapor deposition (CVD) to evenly apply ceramic coating on the surface of EPDM rubber to ceramicize its surface in order to improve the flame retardancy of EPDM rubber. However, this will make the adhesion between EPDM, which has weak adhesion, and the substrate even lower, which will also affect its promotion and use. Therefore, the development of a new type of flame-retardant EPDM rubber is of great significance to the development of the EPDM industry. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a modified diatomite ceramic flame-retardant EPDM rubber composite material and its preparation method and application. The modified diatomite in the raw material of the present invention is rich in active groups and has a large amount of negative charges. It can stably adsorb the flame retardant into its pores and release the flame retardant at a specific temperature to achieve a flame retardant effect; secondly, the present invention also uses acrylic polymer to coat the glass powder to modify it, which can effectively improve the heat resistance of the rubber material. As the temperature of the EPDM rubber composite material increases, the modified glass powder can synergize with the modified diatomite, flame retardant and other fillers to exert a ceramic flame retardant effect, so that the EPDM rubber composite material has good flame retardant performance and its safety is greatly improved, which is of great significance to the development of the EPDM rubber industry.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] A modified diatomite ceramic flame-retardant ethylene propylene rubber composite material comprises 100 parts by weight of ethylene propylene rubber (EPDM), 4.5-5.5 parts by weight of zinc oxide (ZnO), 1.8-2.5 parts by weight of stearic acid (SA), 1.5-2 parts by weight of sulfur (S), 2.1-2.5 parts by weight of tetramethylthiuram disulfide (TMTD), 5-10 parts by weight of paraffin oil, 5-7 parts by weight of montmorillonite, 3-7 parts by weight of talc, 40-50 parts by weight of modified diatomite, 15-20 parts by weight of flame retardant and 15-20 parts by weight of modified glass powder.

[0007] The present invention adopts the modification treatment of fillers diatomaceous earth and glass powder, so that the obtained EPDM rubber composite material has good flame retardant properties. As the temperature of the EPDM rubber composite material increases, the modified diatomaceous earth, modified glass powder, flame retardant and other fillers therein jointly exert a ceramic flame retardant effect, the safety is greatly improved, and it is of great significance to the development of the EPDM industry.

[0008] Furthermore, the preparation method of the modified diatomite comprises the following steps: firstly subjecting the diatomite to plasma treatment, using a high-voltage power supply with a frequency of 400-500 Hz, a pulse width of 10-13 μs, a voltage amplitude of 10-20 kV, and a treatment time of 10-20 min; then pre-treating the diatomite with acid, wherein the pH value of the pre-treatment process is 2-3, and washing; and finally subjecting the diatomite to alkali treatment, wherein the pH value of the alkali treatment process is 10-11, washing, and drying to obtain the modified diatomite.

[0009] When modifying diatomite, the present invention first performs plasma treatment on the diatomite to effectively clean and activate the surface of the diatomite, providing a better basis for subsequent chemical treatment; then acid treatment is performed to increase the silicon-hydrogen bonds and hydroxyl functional groups on the surface of the diatomite; and alkali treatment makes the surface of the diatomite more negatively charged, making it easier to adsorb the flame retardant into its pores and less likely to aggregate or deposit. At the same time, the filling of the flame retardant can effectively improve the compatibility of the diatomite with rubber.

[0010] Furthermore, the average particle size of the modified diatomaceous earth is 0.01-10 microns, and the specific surface area is 200-800m 2 / g.

[0011] Furthermore, the acid is hydrochloric acid or nitric acid; the pretreatment time is 0.5-1.0h, and the pretreatment process is continuously stirred at a stirring speed of 600-800r / min;

[0012] The alkali is sodium hydroxide; the alkali treatment time is 1.5-3.0h, stirring is continued during the alkali treatment process, and the stirring speed is 600-800r / min; ultrasonic operation is performed during the alkali treatment process, and the ultrasonic frequency is 20-80kHz.

[0013] Within the above conditions, the properties of diatomite are modified so that it can better adsorb flame retardant molecules through interactions such as hydrogen bonds, electrostatic effects or van der Waals forces, so that the flame retardant molecules are stably adsorbed on the surface or pores of the diatomite.

[0014] Furthermore, the preparation method of the modified glass powder comprises the following steps: dissolving an acrylic polymer in a solvent to form a solution with a mass fraction of 5-30%, then immersing glass powder in the above solution, respectively adding dibutyltin and a curing agent, stirring at a speed of 500-1000 r / min and ultrasonicating for 15-20 minutes, then volatilizing the solvent, curing, and finally grinding into particles with an average particle size of 10-100 microns to obtain modified glass powder.

[0015] The present invention uses acrylic polymer to coat glass powder, which can not only improve the compatibility of filler and rubber, but also enable the glass powder to be released at a specific temperature, thereby improving the heat resistance of the rubber material and participating in ceramicization under specific conditions, thereby achieving a flame retardant effect.

[0016] When the system temperature rises to 200-300°C, the polymer wrapped around the glass powder in the modified diatomite ceramic flame-retardant EPDM rubber composite material prepared by the present invention begins to thermally decompose and release glass powder. The glass powder released at this stage will significantly improve the high temperature resistance of the EPDM rubber composite material. In particular, when the temperature rises to above 300-400°C, the glass powder begins to soften and form a flame-retardant barrier, providing the first line of protection for the flame retardancy of the EPDM rubber composite material. When the temperature rises to 400-600°C, the modified diatomite enters a weightlessness stage and begins to lose crystal water and adsorbed water. The water vapor formed can reduce the volume percentage of oxygen to form a gaseous barrier. At the same time, the flame retardant cage octaphenyl silsesquioxane (OPS) Or polyphenylsilsesquioxane (POSS) separates from the modified diatomaceous earth and begins to decompose into SiO2, forming a molten layer that acts as a heat insulation and barrier, inhibiting the spread of flames and the combustion of materials, and providing a second line of protection for the flame retardancy of EPDM rubber composites; when the temperature rises to above 600-1000°C, the low-melting-point glass powder and the previously formed SiO2 together form a mobile phase and stick to the surrounding fillers to prevent the fillers from falling off and further burning, and gradually form anhydrous oxides together with the modified diatomaceous earth. Under the action of continuous high temperature, the glass powder, SiI2 and modified diatomaceous earth jointly generate stable SiI2 crystals, which jointly complete the ceramicization of the rubber flame retardant process, and provide a third line of protection for the flame retardancy of EPDM rubber composites.

[0017] Furthermore, the acrylic polymer is acrylic resin; the curing agent is isocyanate; the weight ratio of the acrylic resin, isocyanate and glass powder is 1:(1-1.5):(1-2.5); the amount of dibutyltin is 0.1-0.3% of the acrylic resin.

[0018] Furthermore, the solvent is ethyl acetate or acetone; the ultrasonic frequency is 20-50 kHz; the curing temperature is 30-40° C.; and the curing time is 20-30 min.

[0019] Moreover, the present invention also provides a method for preparing the modified diatomite ceramic flame-retardant EPDM rubber composite material as described above, comprising the following steps:

[0020] ① Dispersing the flame retardant in a solvent, and subjecting it to ultrasonic treatment or mechanical stirring to form a flame retardant dispersion; then immersing the modified diatomaceous earth in the flame retardant dispersion; removing the solvent from the impregnated modified diatomaceous earth and drying it to obtain the modified diatomaceous earth filled with the flame retardant;

[0021] ② Place the EPDM rubber in a double-roll mill, add zinc oxide, stearic acid, sulfur, tetramethylthiuram disulfide, paraffin oil, montmorillonite, talcum powder, the modified diatomaceous earth filled with flame retardant obtained in step ①, and modified glass powder after rolling, and perform triangle packing after all the fillers are added, mix evenly, and then put the sheet down, and vulcanize it on a flat vulcanizer at 160° C. for 15-25 minutes to obtain a modified diatomaceous earth ceramic flame retardant EPDM rubber composite material.

[0022] Furthermore, the solvent is a chlorinated hydrocarbon reagent, and the chlorinated hydrocarbon reagent is preferably chloroform or dichloromethane; the ultrasonic frequency is 30-60kHz; the stirring speed is 600-800r / mmin; the immersion time is 0.5-1.5h; and the drying temperature is 30-50°C.

[0023] Furthermore, the present invention also provides the use of the modified diatomite ceramic flame-retardant EPDM rubber composite material in the preparation of vehicle rubber pipe fittings.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention adopts a modification treatment on the filler diatomaceous earth, so that it is rich in active groups and has a large amount of negative charges, which can stably adsorb the flame retardant into its pores, and effectively improve the compatibility of diatomaceous earth and rubber; secondly, the present invention also adopts polymer-coated glass powder, which can improve the compatibility of the filler and rubber while also improving the heat resistance of the rubber material. As the temperature of the EPDM rubber composite material increases, the modified diatomaceous earth, modified glass powder and flame retardant and other fillers in the material work synergistically to jointly exert a ceramic flame retardant effect, so that the obtained EPDM rubber composite material has good flame retardant properties, which is of great significance to the development of the EPDM rubber EPDM industry.

[0026] 2. The modified diatomite ceramic flame-retardant EPDM rubber composite material provided by the present invention can achieve flame-retardant effect in stages at specific temperatures. Since a large amount of inorganic fillers filled in the rubber greatly improve its heat resistance and thermal stability, the EPDM rubber composite material can maintain a normal working state when the system temperature is lower than 200°C; when the system temperature rises to 200-300°C, the acrylic polymer begins to thermally decompose and release glass powder, which significantly improves the high temperature resistance of the EPDM rubber composite material. In particular, when the temperature rises to above 300-400°C, the glass powder begins to soften and form a flame-retardant barrier, providing the first line of protection for the flame retardancy of the EPDM rubber composite material; when the temperature rises to 400-600°C, the modified silicone The diatomaceous earth begins to lose its crystal water and adsorbed water and forms a gaseous barrier. At the same time, the flame retardant OPS or POSS separates from the modified diatomaceous earth and begins to decompose into SiO2, forming a molten layer that acts as a heat-insulating and barrier layer, and inhibits the spread of flames and the combustion of materials, providing a second line of protection for the flame retardancy of EPDM rubber composites. When the temperature rises to above 600-1000°C, the glass powder and the previously formed SiI2 together form the mobile phase and stick to the surrounding fillers to prevent them from burning. At the same time, the two together with the modified diatomaceous earth form anhydrous oxides, and under the continuous high temperature, they jointly generate SiI2 crystals that tend to be stable, and jointly complete the ceramicization of the rubber in the flame retardant process, providing a third line of protection for the flame retardancy of EPDM rubber composites. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 A flow chart for preparing the modified diatomite ceramic flame-retardant EPDM rubber composite material of the present invention;

[0028] Figure 2 Performance test graphs of oxygen index, tensile strength and dimensional change rate before and after sintering of modified diatomite ceramic flame retardant EPDM rubber composite materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention;

[0029] Figure 3 This is a performance test chart of the elongation at break of the modified diatomite ceramic flame retardant EPDM rubber composite material prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and their accompanying drawings. The embodiments recorded herein are specific embodiments of the present invention, which are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limitations on the embodiments of the present invention and the scope of protection of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims of this application and its specification, including technical solutions that adopt any obvious replacements and modifications to the embodiments recorded herein.

[0031] The reagents used in the present invention are all commonly used reagents and can be purchased from conventional reagent production and sales companies.

[0032] in,

[0033] EPDM rubber, purchased from Dongguan Yucheng Plastic Chemical Co., Ltd., brand number 4570;

[0034] Zinc oxide, CAS No. 1314-13-2;

[0035] Stearic acid, CAS No. 57-11-4;

[0036] Sulfur, CAS No. 7704-34-9;

[0037] Tetramethylthiuram disulfide, CAS No. 137-26-8;

[0038] Paraffin oil, CAS No. 8012-95-1;

[0039] Montmorillonite, CAS No. 1318-93-0;

[0040] Talc, CAS No. 14807-96-6;

[0041] Diatomaceous earth, CAS No. 61790-53-2;

[0042] Glass powder, purchased from Lingshou County Bochuan Mineral Products Processing Plant, mesh number is 1250 mesh;

[0043] Acrylic resin, purchased from Jingyi New Materials, is a hydroxyl functional acrylic resin from Allnex SM548 / 50X;

[0044] Isocyanate, purchased from Jingyi New Materials, is BASF Lupranate MM103C modified isocyanate curing agent;

[0045] Dibutyltin, CAS No. 818-08-6;

[0046] Ethyl acetate, CAS No. 141-78-6;

[0047] Acetone, CAS No. 67-64-1.

[0048] Example 1

[0049] (1) The preparation method of modified diatomite comprises the following steps: firstly, 500g of diatomite is subjected to plasma treatment, the frequency of the high-voltage power supply used is 400Hz, the pulse width is 10μs, the voltage amplitude is 10kV, and the treatment time is 10min; then, the diatomite is pretreated with hydrochloric acid having a mass fraction of 15%, and the pH value of the pretreatment process is 3, that is, the diatomite is immersed in the above acid solution for 0.5h, and the pretreatment process is continuously stirred at a stirring speed of 600r / min. After the treatment, the diatomite is washed with deionized water. The diatomaceous earth is washed until the washing liquid is neutral; finally, 15% by mass sodium hydroxide is used for alkali treatment, and the pH value of the alkali treatment process is 10, that is, the diatomaceous earth is immersed in the above alkali solution for 1.5 hours, and the alkali treatment process is also continuously stirred at a stirring speed of 600r / min. At the same time, ultrasound is also performed during the alkali treatment process, and the ultrasonic frequency is 20kHz. After the treatment, the diatomaceous earth is washed with deionized water until the washing liquid is neutral, and dried to obtain modified diatomaceous earth; the average particle size of the modified diatomaceous earth obtained is 1 micron, and the specific surface area is 200m 2 / g.

[0050] (2) The preparation method of the modified glass powder comprises the following steps: dissolving 100 g of acrylic resin in ethyl acetate to form a 5% mass fraction solution, then immersing the glass powder in the above solution, and then adding dibutyltin and curing agent isocyanate respectively, stirring at a speed of 500 r / min and ultrasonicating for 15 min, the ultrasonic frequency is 20 kHz, then volatilizing the solvent, curing, the curing temperature is 30°C, the curing time is 20 min, and finally grinding into particles with an average particle size of 90 μm to obtain the modified glass powder.

[0051] The weight ratio of the acrylic resin, isocyanate and glass powder is 1:1:1; the amount of dibutyltin is 0.1% of the acrylic resin.

[0052] (3) A method for preparing a modified diatomite ceramic flame-retardant EPDM rubber composite material, comprising the following steps:

[0053] ① Disperse 150g of flame retardant in 1L of chloroform solvent and perform mechanical stirring at a stirring speed of 600r / min to form a flame retardant dispersion; then immerse 400g of modified diatomaceous earth in the flame retardant dispersion for 0.5h; remove the solvent from the impregnated modified diatomaceous earth and dry it at a drying temperature of 30°C to obtain modified diatomaceous earth filled with flame retardant;

[0054] ② Place 1000g of EPDM rubber in a double-roll mill, add 45g of zinc oxide, 18g of stearic acid, 15g of sulfur, 21g of tetramethylthiuram disulfide, 50g of paraffin oil, 50g of montmorillonite, 30g of talc, the modified diatomaceous earth filled with flame retardant obtained in step ①, and 150g of modified glass powder after rolling. After all the fillers are added, a triangle bag operation is performed, mixed evenly, and then the sheet is removed, and vulcanized on a flat vulcanizer at 160°C for 15min to obtain a modified diatomaceous earth ceramic flame retardant EPDM rubber composite material.

[0055] Example 2

[0056] (1) The preparation method of modified diatomite comprises the following steps: firstly, 500g of diatomite is subjected to plasma treatment, the frequency of the high-voltage power supply used is 500Hz, the pulse width is 13μs, the voltage amplitude is 20kV, and the treatment time is 20min; then, the diatomite is pretreated with nitric acid having a mass fraction of 20%, and the pH value of the pretreatment process is 2, that is, the diatomite is immersed in the above acid solution for 1.0h, and the pretreatment process is continuously stirred at a stirring speed of 800r / min; after the treatment, the diatomite is washed with deionized water. The diatomite is treated with sodium hydroxide having a mass fraction of 20%, and the pH value of the alkali treatment process is 11, that is, the diatomite is immersed in the above-mentioned alkali solution for 3.0 hours, and the alkali treatment process is also continuously stirred at a stirring speed of 800r / min. At the same time, the alkali treatment process is also ultrasonically operated at an ultrasonic frequency of 80kHz. After the treatment, the diatomite is washed with deionized water until the washing liquid is neutral, and dried to obtain modified diatomite. The average particle size of the modified diatomite obtained is 0.01 micron, and the specific surface area is 800m 2 / g.

[0057] (2) The preparation method of the modified glass powder comprises the following steps: dissolving 100 g of acrylic resin in solvent acetone to form a solution with a mass fraction of 30%, then immersing glass powder in the above solution, adding dibutyltin and curing agent isocyanate respectively, stirring at a speed of 1000 r / min and ultrasonicating for 20 min at an ultrasonic frequency of 50 kHz, then volatilizing the solvent and curing at a temperature of 40° C. for 30 min, and finally grinding into particles with an average particle size of 35 μm to obtain the modified glass powder.

[0058] The weight ratio of the acrylic resin, isocyanate and glass powder is 1:1.5:2.5; the amount of dibutyl tin is 0.3% of the acrylic resin.

[0059] (3) A method for preparing a modified diatomite ceramic flame-retardant EPDM rubber composite material, comprising the following steps:

[0060] ① Disperse 200g of flame retardant in 1L of dichloromethane solvent and perform ultrasonic treatment at an ultrasonic frequency of 60kHz to form a flame retardant dispersion; then 500g of modified diatomaceous earth is immersed in the flame retardant dispersion; the immersion time is 1.5h; remove the solvent from the impregnated modified diatomaceous earth and dry it at a drying temperature of 50°C to obtain modified diatomaceous earth filled with flame retardant;

[0061] ② Place 1000g of EPDM rubber in a double-roll mill, add 55g of zinc oxide, 25g of stearic acid, 20g of sulfur, 25g of tetramethylthiuram disulfide, 100g of paraffin oil, 70g of montmorillonite, 70g of talc, the modified diatomaceous earth filled with flame retardant obtained in step ①, and 200g of modified glass powder after rolling. After all the fillers are added, a triangle bag operation is performed, mixed evenly, and then the sheet is removed, and vulcanized on a flat vulcanizer at 160°C for 25min to obtain a modified diatomaceous earth ceramic flame retardant EPDM rubber composite material.

[0062] Example 3

[0063] (1) The preparation method of modified diatomite comprises the following steps: firstly, 500g of diatomite is subjected to plasma treatment, the frequency of the high-voltage power supply used is 400Hz, the pulse width is 11μs, the voltage amplitude is 12kV, and the treatment time is 15min; then, the diatomite is pretreated with hydrochloric acid having a mass fraction of 15%, and the pH value of the pretreatment process is 2.5, that is, the diatomite is immersed in the above acid solution for 0.5h, and the pretreatment process is continuously stirred at a stirring speed of 700r / min; after the treatment, the diatomite is washed with deionized water Diatomaceous earth is treated with sodium hydroxide having a mass fraction of 20%, and the pH value of the alkaline treatment process is 10, that is, the diatomaceous earth is immersed in the above alkaline solution for 2.0 hours, and the alkaline treatment process is also continuously stirred at a stirring speed of 700r / min. At the same time, ultrasonic operation is also performed during the alkaline treatment process, and the ultrasonic frequency is 50kHz. After the treatment, the diatomaceous earth is washed with deionized water until the washing liquid is neutral, and dried to obtain modified diatomaceous earth. The average particle size of the modified diatomaceous earth obtained is 0.1 micron, and the specific surface area is 300m 2 / g.

[0064] (2) The preparation method of the modified glass powder comprises the following steps: dissolving 100 g of acrylic resin in solvent acetone to form a solution with a mass fraction of 20%, then immersing glass powder in the above solution, adding dibutyltin and curing agent isocyanate respectively, stirring at a speed of 600 r / min and ultrasonicating for 15 min, the ultrasonic frequency of which is 30 kHz, then volatilizing the solvent, curing at a temperature of 35° C., curing for 20 min, and finally grinding into particles with an average particle size of 50 μm to obtain the modified glass powder.

[0065] The weight ratio of the acrylic resin, isocyanate and glass powder is 1:1:2; the amount of dibutyl tin is 0.2% of the acrylic resin.

[0066] (3) A method for preparing a modified diatomite ceramic flame-retardant EPDM rubber composite material, comprising the following steps:

[0067] ① Disperse 200g of flame retardant in 1L of chloroform and perform ultrasonic treatment at an ultrasonic frequency of 60kHz to form a flame retardant dispersion; then immerse 450g of modified diatomaceous earth in the flame retardant dispersion for 1h; remove the solvent from the impregnated modified diatomaceous earth and dry it at a drying temperature of 30°C to obtain modified diatomaceous earth filled with flame retardant;

[0068] ② Place 1000g of EPDM rubber in a double-roll mill, add 50g of zinc oxide, 21g of stearic acid, 16g of sulfur, 22g of tetramethylthiuram disulfide, 60g of paraffin oil, 50g of montmorillonite, 30g of talcum powder, the modified diatomaceous earth filled with flame retardant obtained in step ①, and 200g of modified glass powder after rolling, and perform a triangle bag operation after all the fillers are added, mix evenly, and then put the sheet down, and vulcanize it on a flat vulcanizer at 160°C for 15-25min to obtain a modified diatomaceous earth ceramic flame retardant EPDM rubber composite material.

[0069] Comparative Example 1

[0070] Comparative Example 1 is similar to Example 3, except that the diatomaceous earth is not modified.

[0071] Comparative Example 2

[0072] Comparative Example 2 is similar to Example 3, except that the diatomaceous earth is not subjected to alkali treatment.

[0073] Comparative Example 3

[0074] Comparative Example 3 is similar to Example 3, except that the glass powder is not modified.

[0075] Comparative Example 4

[0076] Comparative Example 4 is similar to Example 3, except that the amount of dibutyltin used is 0.5% of the acrylic resin; the curing temperature is 75° C., and the curing time is 20 min.

[0077] The performance test of the modified diatomite ceramic flame retardant EPDM rubber composite material provided in the embodiment and the comparative example is carried out, and the specific test process is as follows:

[0078] Refer to GB / T 2408-2008 test to determine the flame retardant level;

[0079] Refer to GB / T2406-1993 to test oxygen index;

[0080] Refer to GB / T528-1998 to test tensile strength and elongation at break;

[0081] High-temperature sintering experiment: Rectangular specimens with a size of 30mm×13mm×1.7mm were then cut from the modified diatomite ceramic flame-retardant EPDM rubber composite sheet and placed in a high-temperature sintering muffle furnace. Finally, they were heated from room temperature to 1000°C at a heating rate of 12°C / min and maintained for 30 minutes for high-temperature sintering. The dimensional change rate before and after sintering and the appearance after sintering were tested.

[0082] The test results are shown in Table 1.

[0083] Table 1 Performance test results of materials

[0084]

[0085] It can be seen from the test results provided in Table 1 that the flame retardant level, oxygen index, tensile strength and elongation at break of the modified diatomite ceramic flame retardant EPDM rubber composite materials prepared by each group of the embodiments of the present invention are better than those of the comparative example, and the dimensional change rate before and after sintering is less than 10%. At the same time, after high-temperature sintering experimental tests, the modified diatomite ceramic flame retardant EPDM rubber composite materials prepared by each group of the embodiments of the present invention are not only ceramicized, but also dense, strong, self-supporting, non-falling, non-cracking and other characteristics. This shows that the present invention uses acid and alkali to modify the filler diatomite, respectively, and successfully makes the filler diatomite absorb the flame retardant into its pores, effectively improving the diatomite and The compatibility of rubber allows diatomaceous earth to be evenly dispersed in the rubber, thereby ensuring that the rubber has excellent properties such as tensile strength and elongation at break, and can present a strong and dense structure during sintering without falling off or cracking, thereby improving the safety of the rubber; secondly, the acrylic polymer modified glass powder of the present invention also improves the compatibility of the filler and the rubber, and while maintaining the excellent properties of the rubber, it also ensures the smooth ceramicization during the sintering process of the rubber, and presents a dense, strong structure that does not fall off or crack, thereby greatly improving the safety of the rubber, so that the obtained EPDM rubber composite material has good flame retardant properties, which is of great significance to the development of the EPDM rubber EPDM industry.

[0086] It can be seen from the test results of Comparative Example 1 that although the rubber material obtained by not modifying the diatomaceous earth also undergoes ceramicization during the sintering process, the dimensional change rate before and after sintering is as high as 27.1%, and the material after sintering shows problems such as looseness, lack of self-support, falling off and cracking, which poses a potential danger. The flame retardant level, oxygen index, tensile strength and elongation at break are also affected to varying degrees.

[0087] It can be seen from the test results of Comparative Example 2 that the diatomaceous earth has not been treated with alkali, thereby reducing the negative charge on its surface and weakening the adsorption capacity of the flame retardant, which also causes a decrease in the flame retardant level, oxygen index, tensile strength and elongation at break. Secondly, it also leads to the discontinuity of the ceramicization process, which makes the sintered material not only loose and non-self-supporting but also cracked, which can easily cause potential dangers.

[0088] From the test results of Comparative Example 3, it can be seen that the failure to modify the glass powder has a certain impact on the dispersibility of the glass powder in the rubber, resulting in varying degrees of decrease in properties such as tensile strength and elongation at break, and the flame retardant level is only V-2, and the oxygen index is only 23.4; in addition, the dimensional change rate before and after sintering is as high as 22.3%, and the material after sintering shows problems of looseness, cracking and falling off, posing certain safety hazards.

[0089] In Comparative Example 4, the process parameters in the glass powder modification process are adjusted, resulting in an increase in the hardness of the modified glass powder particles obtained, which can improve the thermal stability of the rubber material to a certain extent. However, it also increases the thermal decomposition temperature of the polymer wrapped around the modified glass powder particles, resulting in the inability to form a viscous flow bonding and flame retardant barrier inside the rubber material at the initial stage of temperature rise, which affects the flame retardant effect to a certain extent and leads to the discontinuity of the ceramicization process, which in turn causes the rubber material to crack after sintering.

[0090] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A modified diatomite ceramic flame retardant EPDM rubber composite material, characterized in that: The invention comprises 100 parts by weight of EPDM rubber, 4.5-5.5 parts by weight of zinc oxide, 1.8-2.5 parts by weight of stearic acid, 1.5-2 parts by weight of sulfur, 2.1-2.5 parts by weight of tetramethylthiuram disulfide, 5-10 parts by weight of paraffin oil, 5-7 parts by weight of montmorillonite, 3-7 parts by weight of talc, 40-50 parts by weight of modified diatomaceous earth, 15-20 parts by weight of flame retardant and 15-20 parts by weight of modified glass powder.

2. The modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 1, characterized in that: The preparation method of the modified diatomite comprises the following steps: firstly, plasma treatment is performed on the diatomite, the frequency of the high-voltage power supply used is 400-500Hz, the pulse width is 10-13μs, the voltage amplitude is 10-20kV, and the treatment time is 10-20min; then, acid is used to pre-treat the diatomite, the pH value of the pre-treatment process is 2-3, and washing is performed; finally, alkali treatment is performed, the pH value of the alkali treatment process is 10-11, washing and drying are performed to obtain the modified diatomite.

3. The modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 2, characterized in that: The modified diatomaceous earth has an average particle size of 0.01-10 microns and a specific surface area of ​​200-800 m 2 / g.

4. The modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 2, characterized in that: The acid is hydrochloric acid or nitric acid; the pretreatment time is 0.5-1.0h, and the pretreatment process is continuously stirred at a stirring speed of 600-800r / min; The alkali is sodium hydroxide; the alkali treatment time is 1.5-3.0h, stirring is continued during the alkali treatment process, and the stirring speed is 600-800r / min; ultrasonic operation is performed during the alkali treatment process, and the ultrasonic frequency is 20-80kHz.

5. The modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 1, characterized in that: The preparation method of the modified glass powder comprises the following steps: dissolving an acrylic polymer in a solvent to form a solution with a mass fraction of 5-30%, then soaking glass powder in the solution, respectively adding dibutyltin and a curing agent, stirring at a speed of 500-1000 r / min and ultrasonicating for 15-20 minutes, then volatilizing the solvent, curing, and finally grinding into particles with an average particle size of 10-100 microns to obtain the modified glass powder.

6. The modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 5, characterized in that: The acrylic polymer is acrylic resin; the curing agent is isocyanate; the weight ratio of the acrylic resin, isocyanate and glass powder is 1:(1-1.5):(1-2.5); the amount of dibutyltin is 0.1-0.3% of the acrylic resin.

7. The modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 5, characterized in that: The solvent is ethyl acetate or acetone; the ultrasonic frequency is 20-50 kHz; the curing temperature is 30-40° C., and the curing time is 20-30 min.

8. The method for preparing the modified diatomite ceramic flame-retardant EPDM rubber composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: ① Dispersing the flame retardant in the solvent and subjecting it to ultrasonic treatment or mechanical stirring to form a flame retardant dispersion; Then, the modified diatomaceous earth is immersed in the flame retardant dispersion; the solvent is removed from the immersed modified diatomaceous earth and then dried to obtain the modified diatomaceous earth filled with the flame retardant; ② Place the EPDM rubber in a double-roll mill, add zinc oxide, stearic acid, sulfur, tetramethylthiuram disulfide, paraffin oil, montmorillonite, talcum powder, the modified diatomaceous earth filled with flame retardant obtained in step ①, and modified glass powder after rolling, and perform triangle packing after all the fillers are added, mix evenly, and then put the sheet down, and vulcanize it on a flat vulcanizer at 160° C. for 15-25 minutes to obtain a modified diatomaceous earth ceramic flame retardant EPDM rubber composite material.

9. The method for preparing the modified diatomite ceramic flame-retardant EPDM rubber composite material according to claim 8, characterized in that: The solvent is a chlorinated hydrocarbon reagent; the ultrasonic frequency is 30-60kHz; the stirring speed is 600-800r / min; the immersion time is 0.5-1.5h; and the drying temperature is 30-50°C.

10. Use of the modified diatomite ceramic flame-retardant EPDM rubber composite material according to any one of claims 1 to 7 in the preparation of vehicle rubber pipe fittings.