Electromagnetic shielding PMMA composite board material and preparation method thereof

By introducing specific components and processes into PMMA composite boards, PMMA composite boards with both excellent electromagnetic shielding and flame retardant properties are prepared, solving the problem of insufficient electromagnetic shielding and flame retardant properties of existing acrylic sheets and improving the overall performance of the material.

CN118879014AActive Publication Date: 2024-11-01ZHEJIANG LONGYOU ZHANYU ACRYLIC

Patent Information

Application Number
CN202411129091.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

Existing antibacterial and flame-retardant acrylic sheets have insufficient electromagnetic shielding and flame-retardant properties, posing electromagnetic interference and fire safety hazards.

Method used

PMMA composite materials, composed of pentaerythritol phosphate, nano-titanium dioxide, zirconium phosphate, electromagnetic shielding agent, flame retardant, antistatic agent and lubricant, are used to prepare electromagnetic shielding PMMA composite plates through a specific process. The electromagnetic shielding performance is improved by the synergistic effect of graphene oxide and metal complex salt oxide, and the flame retardant performance is improved by the reaction of 1,4-diaminobenzene and phenylphosphonic acid.

Benefits of technology

The prepared PMMA composite board material possesses both excellent electromagnetic shielding and flame retardant properties, thus improving the material's quality and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997312120000091
    Figure BDA0004997312120000091
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, in particular to an electromagnetic shielding PMMA composite board material and a preparation method thereof. The electromagnetic shielding PMMA composite board material is prepared from the following raw materials in parts by weight: 90 to 110 parts of methyl methacrylate, 3 to 5 parts of pentaerythritol phosphate, 0.6 to 1.2 parts of simethicone, 4 to 7 parts of nano titanium dioxide, 2 to 3 parts of zirconium phosphate, 0.5 to 0.8 part of initiator, 5 to 8 parts of electromagnetic shielding agent, 2 to 3 parts of flame-retardant aid, 3 to 6 parts of antistatic agent, 2 to 5 parts of lubricant and 3 to 6 parts of pigment. The PMMA composite board material prepared by the invention not only has excellent electromagnetic shielding performance, but also has excellent flame retardant property, and the grade and quality of the PMMA composite board material are effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to an electromagnetic shielding PMMA composite plate material and a preparation method thereof. Background Art

[0002] Acrylic sheet is polymethyl methacrylate (PMMA) sheet, which is polymerized from "methyl methacrylate (MMA)". Or it is extruded from acrylic pellets through an extruder. In the past, the sheet was commonly known as plexiglass. Acrylic comes from the English word acrylic, which means PMMA sheet made of organic compound MMA, which is as transparent and transparent as glass. All sheets made of transparent plastics such as PS, PC, etc. or from inferior recycled MMA are collectively called plexiglass. Because acrylic has good transparency, chemical stability and weather resistance, is easy to dye, easy to process, and has a beautiful appearance, it is widely used in the construction industry.

[0003] In the patent document with application number "CN201610409978.2", an antibacterial flame-retardant acrylic sheet and a preparation method thereof are disclosed. The antibacterial flame-retardant acrylic sheet is prepared from the following raw materials in parts by weight: 95-105 parts of methyl methacrylate, 0.1-0.7 parts of dibenzoyl peroxide, 15-25 parts of magnesium hydroxide, 0.1-0.5 parts of dimethyl silicone oil, 1-5 parts of inorganic antibacterial agent, and 0.5-1.5 parts of antistatic agent. Although the acrylic sheet prepared in this patent document has certain flame retardant properties and excellent antibacterial properties, its own anti-electromagnetic shielding performance is relatively poor. Nowadays, electromagnetic radiation pollution has become a new environmental pollution, which not only causes serious interference to daily communication equipment, computers and other electronic systems, but also poses a serious threat to information security, and also brings immeasurable damage to human health. Furthermore, its flame retardant performance is relatively insufficient, and fire may occur. There are certain safety hazards, which still need to be further improved. Based on this, the present invention provides an electromagnetic shielding PMMA composite plate material and a preparation method thereof, which has solved the above-mentioned technical problems! Summary of the invention

[0004] The purpose of the present invention is to provide an electromagnetic shielding PMMA composite plate material and a preparation method thereof. The prepared PMMA composite plate material not only has excellent electromagnetic shielding performance, but also has excellent flame retardant performance, effectively ensuring its grade and quality.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] The invention discloses an electromagnetic shielding PMMA composite plate material, which is composed of the following raw materials in parts by weight: 90 to 110 parts of methyl methacrylate, 3 to 5 parts of pentaerythritol phosphate, 0.6 to 1.2 parts of dimethyl silicone oil, 4 to 7 parts of nano titanium dioxide, 2 to 3 parts of zirconium phosphate, 0.5 to 0.8 parts of initiator, 5 to 8 parts of electromagnetic shielding agent, 2 to 3 parts of flame retardant additive, 3 to 6 parts of antistatic agent, 2 to 5 parts of lubricant and 3 to 6 parts of pigment.

[0007] Furthermore, the initiator is selected from any one of dibenzoyl peroxide, diisobutyryl peroxide, and isopropylphenyl peroxide neodecanoate.

[0008] Furthermore, the preparation method of the electromagnetic shielding agent is: adding cobalt chloride with a mass of 0.6 to 0.7 times that of ferric chloride to a 0.02 to 0.05 g / mL ferric chloride aqueous solution, adding graphene oxide aqueous dispersion to the obtained mixed solution after mixing and stirring evenly, adjusting the pH to 10.5 to 11.5 after ultrasonic dispersion for 30 to 40 minutes, and then adding sodium thiosulfate with a molar amount of 0.3 to 0.4 times that of ferric chloride, mixing evenly and sealing, and heating the reaction at a temperature of 130 to 170° C. for 20 to 40 hours; after the reaction is completed, naturally cooling it to room temperature, and then centrifuging and washing and drying the obtained product components in turn to obtain the electromagnetic shielding agent.

[0009] Furthermore, the concentration of graphene oxide in the graphene oxide aqueous dispersion is 10-20 g / L, and its usage is 5-8% of the volume of the mixed solution.

[0010] Furthermore, the preparation method of the flame retardant additive comprises the following steps: adding 1,4-diaminobenzene into anhydrous ethanol at a dosage ratio of 0.15 to 0.25 mol / L, mixing and stirring under nitrogen protection to completely dissolve it, then adding phenylphosphonic acid with a molar amount of 0.8 to 1.2 times that of 1,4-diaminobenzene to the obtained mixed components, mixing and stirring evenly, and then reflux reacting for 3 to 5 hours; after the reaction is completed, naturally cooling the obtained product components to room temperature, and continuing to stir and react for 6 to 10 hours at room temperature; after the reaction is completed, the obtained reaction product is separated into solid and liquid, and then the obtained solid filter material is washed with anhydrous ethanol until the obtained filtrate is a colorless and transparent liquid, and the washed solid material is then vacuum dried to obtain the flame retardant additive.

[0011] Furthermore, the vacuum drying temperature is set to 70-80° C., and the vacuum drying time is set to 10-12 hours.

[0012] Furthermore, the antistatic agent is selected from one of N-hydroxymethyl acrylamide, N-(2-hydroxypropyl) methacrylamide and N-hydroxymethyl acrylamide.

[0013] Furthermore, the lubricant is selected from any one of stearic acid, polyethylene wax, ethylene bisstearamide, and silicone powder.

[0014] Furthermore, the pigment is selected from any one of chrome yellow, black iron oxide and red iron oxide.

[0015] A method for preparing an electromagnetic shielding PMMA composite plate material comprises the following steps:

[0016] Step 1, accurately weigh each raw material according to the formula, then add methyl methacrylate and initiator into the reactor, mix and stir evenly, and heat and polymerize in a water bath at 80-85° C. for 30-40 minutes;

[0017] Step 2: After the reaction is completed, the resulting product components are naturally cooled to room temperature, and then the remaining raw materials are added, mixed and stirred evenly, and the resulting mixed slurry is poured into the corresponding mold, and then subjected to air bath heating polymerization, cooling and demolding treatment in sequence to obtain an electromagnetic shielding PMMA composite board material.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention puts cobalt chloride into an aqueous solution of ferric chloride, mixes and stirs evenly, then adds graphene oxide aqueous phase dispersion and sodium thiosulfate, mixes and stirs evenly, heats it, makes it undergo redox reaction, and obtains electromagnetic shielding agent after centrifugal washing and drying treatment. The obtained electromagnetic shielding agent is composed of metal complex salt oxide and graphene with excellent conductivity, and the two cooperate and cooperate with each other, effectively ensuring the electromagnetic shielding performance of PMMA composite plate material. Furthermore, the present invention puts 1,4-diaminobenzene into anhydrous ethanol, then adds phenylphosphonic acid thereto, mixes and stirs evenly, and refluxes to react, after the reaction is completed, cools and continues to stir the reaction treatment, and then sequentially performs solid-liquid separation, washing and vacuum drying treatment on the obtained reaction product, and finally obtains a flame retardant additive. The prepared flame retardant additive can significantly improve the flame retardant performance of PMMA composite plate material, and effectively improves its quality. In summary, the PMMA composite plate material prepared by the present invention not only has excellent electromagnetic shielding performance, but also has excellent flame retardant performance, effectively ensuring its grade and quality. DETAILED DESCRIPTION

[0020] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] An electromagnetic shielding PMMA composite plate material is composed of the following raw materials in parts by weight: 90 parts of methyl methacrylate, 3 parts of pentaerythritol phosphate, 0.6 parts of dimethyl silicone oil, 4 parts of nano titanium dioxide, 2 parts of zirconium phosphate, 0.5 parts of dibenzoyl peroxide, 5 parts of electromagnetic shielding agent, 2 parts of flame retardant additive, 3 parts of N-hydroxymethyl acrylamide, 2 parts of stearic acid and 3 parts of chrome yellow.

[0023] The preparation method of the electromagnetic shielding agent is as follows: add cobalt chloride whose mass is 0.6 times of the ferric chloride to a 0.02g / mL ferric chloride aqueous solution, mix and stir evenly, add graphene oxide aqueous dispersion to the obtained mixed solution, adjust the pH to 10.5 after ultrasonic dispersion for 30 minutes, then add sodium thiosulfate whose molar amount is 0.3 times of the ferric chloride, mix evenly and seal, and heat to react at a temperature of 130°C for 20 hours; after the reaction is completed, cool it naturally to room temperature, and then centrifuge and wash and dry the obtained product components in turn to obtain the electromagnetic shielding agent; wherein, the concentration of graphene oxide in the graphene oxide aqueous dispersion is 10g / L, and its amount is 5% of the volume of the mixed solution.

[0024] The preparation method of the flame retardant additive comprises the following steps: adding 1,4-diaminobenzene into anhydrous ethanol at a dosage ratio of 0.15 mol / L, mixing and stirring under nitrogen protection to completely dissolve the mixture, then adding phenylphosphonic acid with a molar amount of 0.8 times that of 1,4-diaminobenzene to the obtained mixed components, mixing and stirring evenly, and then reflux reacting for 3 hours; after the reaction is completed, naturally cooling the obtained product components to room temperature, and continuing to stir and react for 6 hours under room temperature conditions; after the reaction is completed, performing solid-liquid separation on the obtained reaction product, and then washing the obtained solid filter material with anhydrous ethanol until the obtained filtrate is a colorless and transparent liquid, and the washed solid material is then vacuum dried to obtain the flame retardant additive; wherein the vacuum drying temperature is set to 70°C, and the vacuum drying time is set to 10 hours.

[0025] A method for preparing an electromagnetic shielding PMMA composite plate material comprises the following steps:

[0026] Step 1: accurately weigh the raw materials according to the formula, then add methyl methacrylate and initiator into the reactor, mix and stir evenly, and heat and polymerize in a water bath at 80° C. for 30 minutes;

[0027] Step 2: After the reaction is completed, the resulting product components are naturally cooled to room temperature, and then the remaining raw materials are added, mixed and stirred evenly, and the resulting mixed slurry is poured into the corresponding mold, and then heated and polymerized in an air bath, cooled and demolded to obtain an electromagnetic shielding PMMA composite board material.

[0028] Example 2

[0029] The preparation method of an electromagnetic shielding PMMA composite plate material provided in this embodiment is basically the same as that in Example 1, except that the specific composition of the raw materials used and the preparation methods of the electromagnetic shielding agent and the flame retardant additive are not completely the same, and the specific composition of the raw materials used in this embodiment and the preparation methods of the electromagnetic shielding agent and the flame retardant additive are as follows:

[0030] An electromagnetic shielding PMMA composite plate material is composed of the following raw materials in parts by weight: 100 parts of methyl methacrylate, 4 parts of pentaerythritol phosphate, 1.0 part of dimethyl silicone oil, 5 parts of nano titanium dioxide, 2.5 parts of zirconium phosphate, 0.6 parts of diisobutyryl peroxide, 6 parts of electromagnetic shielding agent, 2.5 parts of flame retardant additive, 4 parts of N-(2-hydroxypropyl) methacrylamide, 3 parts of polyethylene wax and 5 parts of black iron oxide.

[0031] The preparation method of the electromagnetic shielding agent is as follows: add cobalt chloride whose mass is 0.65 times of the ferric chloride to a 0.03 g / mL ferric chloride aqueous solution, mix and stir evenly, add graphene oxide aqueous dispersion to the obtained mixed solution, adjust the pH to 11 after ultrasonic dispersion for 35 minutes, then add sodium thiosulfate whose molar amount is 0.35 times of the ferric chloride, mix evenly and seal, and heat to react at a temperature of 150°C for 30 hours; after the reaction is completed, cool it naturally to room temperature, and then centrifuge and wash and dry the obtained product components in turn to obtain the electromagnetic shielding agent; wherein, the concentration of graphene oxide in the graphene oxide aqueous dispersion is 15 g / L, and its amount is 6% of the volume of the mixed solution.

[0032] The preparation method of the flame retardant additive comprises the following steps: adding 1,4-diaminobenzene into anhydrous ethanol at a dosage ratio of 0.2 mol / L, mixing and stirring to completely dissolve the mixture under nitrogen protection, then adding phenylphosphonic acid in an equal molar amount to 1,4-diaminobenzene to the obtained mixed components, mixing and stirring evenly, and then reflux reacting for 4 hours; after the reaction is completed, naturally cooling the obtained product components to room temperature, and continuing to stir and react for 8 hours under room temperature conditions; after the reaction is completed, performing solid-liquid separation on the obtained reaction product, and then washing the obtained solid filter material with anhydrous ethanol until the obtained filtrate is a colorless transparent liquid, and the washed solid material is then vacuum dried to obtain the flame retardant additive; wherein the vacuum drying temperature is set to 75°C, and the vacuum drying time is set to 12 hours.

[0033] Example 3

[0034] The preparation method of an electromagnetic shielding PMMA composite plate material provided in this embodiment is basically the same as that in Example 1, except that the specific composition of the raw materials used and the preparation methods of the electromagnetic shielding agent and the flame retardant additive are not completely the same, and the specific composition of the raw materials used in this embodiment and the preparation methods of the electromagnetic shielding agent and the flame retardant additive are as follows:

[0035] The invention discloses an electromagnetic shielding PMMA composite plate material, which is composed of the following raw materials in parts by weight: 110 parts of methyl methacrylate, 5 parts of pentaerythritol phosphate, 1.2 parts of dimethyl silicone oil, 7 parts of nano titanium dioxide, 3 parts of zirconium phosphate, 0.8 parts of cumyl peroxy neodecanoate, 8 parts of electromagnetic shielding agent, 3 parts of flame retardant additive, 6 parts of N-hydroxymethyl acrylamide, 5 parts of ethylene bisstearamide and 6 parts of red iron oxide.

[0036] The preparation method of the electromagnetic shielding agent is as follows: add cobalt chloride whose mass is 0.7 times of the ferric chloride to a 0.05 g / mL ferric chloride aqueous solution, mix and stir evenly, add graphene oxide aqueous dispersion to the obtained mixed solution, adjust the pH to 11.5 after ultrasonic dispersion for 40 minutes, then add sodium thiosulfate whose molar amount is 0.4 times of the ferric chloride, mix evenly and seal, and heat to react at a temperature of 170°C for 40 hours; after the reaction is completed, cool it naturally to room temperature, and then centrifuge and wash and dry the obtained product components in sequence to obtain the electromagnetic shielding agent; wherein, the concentration of graphene oxide in the graphene oxide aqueous dispersion is 20 g / L, and its amount is 8% of the volume of the mixed solution.

[0037] The preparation method of the flame retardant additive comprises the following steps: adding 1,4-diaminobenzene into anhydrous ethanol at a dosage ratio of 0.25 mol / L, mixing and stirring under nitrogen protection to make it completely dissolved, then adding phenylphosphonic acid with a molar amount of 1.2 times that of 1,4-diaminobenzene to the obtained mixed components, mixing and stirring evenly, and then reflux reaction for 5 hours; after the reaction is completed, naturally cooling the obtained product components to room temperature, and continuing to stir and react for 10 hours under room temperature conditions; after the reaction is completed, performing solid-liquid separation on the obtained reaction product, and then washing the obtained solid filter material with anhydrous ethanol until the obtained filtrate is a colorless and transparent liquid, and the washed solid material is then vacuum dried to obtain the flame retardant additive; wherein the vacuum drying temperature is set to 80°C, and the vacuum drying time is set to 12 hours.

[0038] Comparative Example 1: The difference between this embodiment and embodiment 1 is that this embodiment does not contain an electromagnetic shielding agent.

[0039] Comparative Example 2: The difference between this embodiment and embodiment 1 is that this embodiment does not contain a flame retardant additive.

[0040] Performance test: The relevant properties of the PMMA composite plate material samples provided in Examples 1 to 3 and Comparative Examples 1 to 2 were tested respectively, and the obtained test data were recorded in the following table:

[0041]

[0042] By comparing and analyzing the relevant data in the table, it can be seen that the PMMA composite plate material prepared by the present invention not only has excellent electromagnetic shielding performance, but also has excellent flame retardant performance, effectively ensuring its grade and quality. This shows that the electromagnetic shielding PMMA composite plate material and the preparation method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.

[0043] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0044] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. An electromagnetic shielding PMMA composite plate material, It is characterized in that The invention is composed of the following raw materials in parts by weight: 90-110 parts of methyl methacrylate, 3-5 parts of pentaerythritol phosphate, 0.6-1.2 parts of dimethyl silicone oil, 4-7 parts of nano titanium dioxide, 2-3 parts of zirconium phosphate, 0.5-0.8 parts of initiator, 5-8 parts of electromagnetic shielding agent, 2-3 parts of flame retardant additive, 3-6 parts of antistatic agent, 2-5 parts of lubricant and 3-6 parts of pigment.

2. The electromagnetic shielding PMMA composite plate material according to claim 1, Features: The initiator is selected from any one of dibenzoyl peroxide, diisobutyryl peroxide, and cumyl peroxide neodecanoate.

3. The electromagnetic shielding PMMA composite plate material according to claim 1, It is characterized in that The preparation method of the electromagnetic shielding agent is as follows: adding cobalt chloride whose mass is 0.6-0.7 times of the iron chloride into a 0.02-0.05 g / mL iron chloride aqueous solution, mixing and stirring evenly, adding graphene oxide aqueous phase dispersion to the obtained mixed solution, ultrasonically dispersing for 30-40 minutes, adjusting the pH value to 10.5-11.5, then adding sodium thiosulfate whose molar amount is 0.3-0.4 times of the iron chloride, mixing evenly and sealing, and heating at a temperature of 130-170° C. for reaction for 20-40 hours; after the reaction is completed, naturally cooling to room temperature, and then centrifugally washing and drying the obtained product components in sequence to obtain the electromagnetic shielding agent.

4. The electromagnetic shielding PMMA composite plate material according to claim 3, Features: The concentration of graphene oxide in the graphene oxide aqueous phase dispersion is 10-20 g / L, and its usage is 5-8% of the volume of the mixed solution.

5. The electromagnetic shielding PMMA composite plate material according to claim 1, It is characterized in that The preparation method of the flame retardant auxiliary agent comprises the following steps: adding 1,4-diaminobenzene into anhydrous ethanol at a dosage ratio of 0.15-0.25 mol / L, mixing and stirring to completely dissolve the 1,4-diaminobenzene under nitrogen protection, then adding phenylphosphonic acid with a molar amount of 0.8-1.2 times that of 1,4-diaminobenzene to the obtained mixed components, mixing and stirring evenly, and then reflux reaction for 3-5 hours; after the reaction is completed, naturally cooling the obtained product components to room temperature, and continuing to stir and react for 6-10 hours under room temperature; after the reaction is completed, performing solid-liquid separation on the obtained reaction product, and then washing the obtained solid filter material with anhydrous ethanol until the obtained filtrate is a colorless transparent liquid, and then performing vacuum drying on the washed solid material to obtain the flame retardant auxiliary agent.

6. The electromagnetic shielding PMMA composite plate material according to claim 5, Features: The vacuum drying temperature is set to 70-80° C., and the vacuum drying time is set to 10-12 hours.

7. The electromagnetic shielding PMMA composite plate material according to claim 1, Features: The antistatic agent is selected from one of N-hydroxymethyl acrylamide, N-(2-hydroxypropyl) methacrylamide and N-hydroxymethyl acrylamide.

8. The electromagnetic shielding PMMA composite plate material according to claim 1, Features: The lubricant is selected from any one of stearic acid, polyethylene wax, ethylene bis stearamide and silicone powder.

9. The electromagnetic shielding PMMA composite plate material according to claim 1, Features: The pigment is selected from any one of chrome yellow, black iron oxide and red iron oxide.

10. A method for preparing an electromagnetic shielding PMMA composite plate material according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Step 1, accurately weigh each raw material according to the formula, then add methyl methacrylate and initiator into the reactor, mix and stir evenly, and heat and polymerize in a water bath at 80-85° C. for 30-40 minutes; Step 2: After the reaction is completed, the resulting product components are naturally cooled to room temperature, and then the remaining raw materials are added, mixed and stirred evenly, and the resulting mixed slurry is poured into the corresponding mold, and then subjected to air bath heating polymerization, cooling and demolding treatment in sequence to obtain an electromagnetic shielding PMMA composite board material.

Citation Information

Patent Citations

  • Flame-retardant polymethyl methacrylate

    CN104045955A

  • Composite board based on PMMA / PC and preparation method and application thereof

    CN111823675A

  • Colored heat-resistant and flame-retardant polymethyl methacrylate composite material and preparation method thereof

    CN111925474A

  • Anti-electromagnetic interference liquid crystal display screen

    CN114063334A

  • Preparation method of antibacterial flame-retardant acrylic bathroom panel

    CN114479331A

Cited By

  • Shielding glass and preparation method thereof

    CN119369744A

  • High-permeability low-halogen LED-UV (Light Emitting Diode-Ultraviolet) curing rotary blue ink

    CN119570308A