Unidirectional conductive rubber material as well as preparation method and application thereof

Through the combination of modified conductive particles and rubber matrix and dry modification process, the conductive network discontinuity and easy oxidation problems of traditional conductive rubber materials are solved, and the unidirectional conductive performance and electromagnetic shielding performance are improved, and the material density is reduced and production costs.

CN118879082APending Publication Date: 2024-11-01陕西华秦科技实业股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124807.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Traditional conductive rubber materials have problems such as easy oxidation of metal fillers, resulting in electrical performance decay, discontinuity of conductive networks, difficulty in meeting the unidirectional conductive demand, and high filler content leads to reduced strength, increased density and increased cost.

Method used

Using a specific weight ratio of modified conductive particles and rubber matrix with vulcanizing agent, an electromagnetic coupling hybrid network is constructed through a dry modification process to improve the interface compatibility between fillers and rubber matrix, meet the unidirectional conductive needs, and be modified through surface Sexual treatment delays the oxidation reaction.

Benefits of technology

It achieves the stability and service life of the conductive properties, meets the characteristics of unidirectional conductivity, and reduces material density and production costs, providing excellent electromagnetic shielding and mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of composite high polymer materials, and particularly discloses a one-way conductive rubber material and a preparation method and application thereof.The one-way conductive rubber material is prepared from, by weight, 100 parts of a rubber matrix, 1-5 parts of a vulcanizing agent and 150-300 parts of modified conductive particles, the modified conductive particles are obtained by treating conductive particles through prepared coupling agent modification liquid or a coupling agent. Wherein when the coupling agent modified liquid is prepared, a coupling agent, absolute ethyl alcohol and deionized water are fully and evenly mixed according to the weight ratio, then stirring is continuously conducted in the process of adding acetic acid, the pH value is adjusted to 4-5, and therefore preparation of the coupling agent modified liquid is completed, and the weight ratio of the coupling agent to the conductive particles is (0.5-5): 100. The unidirectional conductive rubber material provided by the invention not only has conductivity in the Z-axis direction and is in an insulating state in the X-axis direction and the Y-axis direction, but also has excellent mechanical properties and electromagnetic shielding properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite polymer materials, and in particular relates to a unidirectional conductive rubber material and a preparation method and application thereof. Background Art

[0002] In the field of electronic technology, conductive rubber is an important composite functional material with an increasingly wide range of applications. Traditional conductive rubber products are usually made of rubber matrix materials and various conductive fillers (including metal silver powder, carbon black, silver-plated aluminum powder, nickel-plated graphite powder, etc.) and other additives. Among them, metal filler-filled conductive rubber has relatively excellent electrical properties (volume resistivity can reach 10 -2 Ω·cm~10 -3 Ω·cm), and is widely used in many high-end fields such as electronic communications (commonly used in connectors, antennas, etc. to ensure stable signal transmission), aerospace (used for spacecraft electronic equipment to ensure the normal operation of the system).

[0003] However, the existing metal filler filled conductive rubber has the following defects:

[0004] For the first time, once metal fillers are exposed to air or in a high temperature environment, they are very likely to undergo oxidation reactions. This chemical reaction will gradually change the physical and chemical properties of the metal fillers, causing their conductivity to gradually decline, and then the overall electrical properties of the conductive rubber will be significantly reduced as the use time continues to increase. This is undoubtedly a serious problem for those application scenarios that require extremely high electrical performance stability, such as long-term electronic equipment or aerospace components working in harsh environments.

[0005] Secondly, the conductive network formed by the overlapping of these conductive particles is not perfectly continuous. At the microscopic level, there are many discontinuities and gaps, which greatly limit the free transmission of current and make it difficult for the conductivity of conductive rubber to reach the excellent level of metal. This discontinuity not only affects the performance of conductive rubber in special application scenarios such as high current and high frequency, but also limits its application in more sophisticated and demanding electronic devices.

[0006] Furthermore, the isotropic conductivity of traditional conductive rubber is insufficient in many specific applications. In application scenarios where the current direction needs to be strictly controlled and unidirectional conductivity is required, it cannot meet actual needs. This limitation is particularly prominent in some electronic devices that have strict requirements on electromagnetic compatibility and signal transmission direction, which may cause signal interference, energy loss and other problems, seriously affecting the performance and reliability of the equipment.

[0007] Finally, in order to achieve specific conductive performance indicators, a large amount of conductive fillers need to be added, and their mass content is usually between 60% and 90%. Such a high proportion of filler addition brings a series of negative problems to conductive rubber. On the one hand, a large amount of conductive fillers greatly reduces the strength of the rubber, making it difficult to withstand large mechanical stress and impact; on the other hand, the high filler content leads to a significant increase in the density of the rubber and an increase in hardness, making the rubber material bulky and lacking in flexibility, while also greatly increasing the production cost, limiting its wide application in some weight- and cost-sensitive application fields.

[0008] For example, the Chinese patent number CN112322043A provides a conductive rubber material with wide frequency range and high efficiency. Although it performs well in electromagnetic shielding performance, when facing a precision chassis that needs to be connected with fine spacing, due to its isotropic conductive properties, it is very easy to damage adjacent fine circuits, thereby causing damage to components.

[0009] In view of this, this invention is proposed. Summary of the invention

[0010] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a unidirectional conductive rubber material and a preparation method and application thereof, so as to solve the problems existing in traditional conductive rubber, such as the metal filler is easily oxidized and the electrical performance decays over time, the discontinuity of the conductive network affects the conductivity, the isotropy is difficult to meet the unidirectional conductivity requirements, and the high filler content causes the rubber strength to decrease, the density to increase, the hardness to increase and the cost to increase.

[0011] In order to achieve the above object, the present invention adopts the following technical solutions:

[0012] In a first aspect, the present invention provides a unidirectional conductive rubber material, which comprises the following raw materials by weight: 100 parts of a rubber matrix, 1 to 5 parts of a vulcanizing agent, and 150 to 300 parts of modified conductive particles;

[0013] The modified conductive particles are prepared by preparing a coupling agent modification liquid or by modifying the surface of the conductive particles with a coupling agent; wherein, when preparing the coupling agent modification liquid, the coupling agent, anhydrous ethanol and deionized water are firstly mixed uniformly according to a set weight ratio, and then continuously stirred during the addition of acetic acid, and the pH value is adjusted to 4-5, thereby completing the preparation of the coupling agent modification liquid.

[0014] That is to say, the weight ratio of the rubber matrix, the vulcanizing agent and the modified conductive particles in the present invention is 100: (1-5): (150-300). Preferably, the weight ratio of the rubber matrix, the vulcanizing agent and the modified conductive particles is 100: (1-3): (150-300); more preferably, the weight ratio of the rubber matrix, the vulcanizing agent and the modified conductive particles is 100: (1-3): (180-220).

[0015] Furthermore, when preparing the modified conductive particles, the coupling agent modification liquid or coupling agent is evenly disposed on the surface of the conductive particles and stirred at the same time, generally for 10 minutes to 30 minutes, and then dried, generally at 60°C to 130°C for 1 hour to 3 hours, to obtain the modified conductive particles.

[0016] The coupling agent modification liquid or coupling agent can be evenly disposed on the surface of the conductive particles in a suitable manner, for example, the coupling agent modification liquid or coupling agent can be distributed on the surface of the conductive particles by spraying.

[0017] The present invention adopts a dry modification process to modify the conductive particles of the functional filler, which greatly improves the interface compatibility between the filler and the rubber matrix, effectively solves the problem of filler agglomeration, and constructs an electromagnetic coupling hybrid network in the rubber matrix, thus solving the bottleneck problem that conventional methods are difficult to achieve both high conductivity and magnetic conductivity and excellent mechanical properties of polymer composite materials.

[0018] Furthermore, when preparing the coupling agent modified liquid, the weight ratio of the coupling agent, deionized water and anhydrous ethanol is (20-30): (5-8): (65-72).

[0019] Furthermore, the coupling agents mentioned above are all selected from silane coupling agents, and the weight ratio of the coupling agents to the conductive particles is (0.5-5): 100. Preferably, the weight ratio of the coupling agents to the conductive particles is (1-3): 100; more preferably, the weight ratio of the coupling agents to the conductive particles is (1-2): 100.

[0020] Specifically, the silane coupling agent can be KH550, A-171, A-151, KH560 or KH570 produced by Jiangxi Chenguang New Materials Co., Ltd.

[0021] Furthermore, the conductive particles are any one of silver-plated copper particles, silver-plated aluminum particles, silver-plated glass particles or gold-nickel coated styrene particles, and the particle size range of the conductive particles is 10μm to 50μm; preferably, the particle size range of the conductive particles is 20μm to 50μm; more preferably, the particle size range of the conductive particles is 40μm to 50μm.

[0022] Furthermore, the rubber matrix is ​​selected from any one or more combinations of silicone rubber, fluorosilicone rubber and borosilicate rubber.

[0023] Furthermore, the vulcanizing agent is selected from any one or more combinations of dicumyl peroxide, dibenzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane.

[0024] In a second aspect, the present invention also provides a method for preparing the above-mentioned unidirectional conductive rubber material, wherein the rubber matrix, the vulcanizing agent and the modified conductive particles are first placed on an open mill and fully mixed until they are uniform, thereby obtaining a mixed rubber material; the mixed rubber material is then vulcanized to obtain the unidirectional conductive rubber material.

[0025] The mixing can be carried out in a manner commonly used in the art. Preferably, the number of triangle packing is not less than 8 times during the mixing process, and the mixing time is not less than 30 minutes.

[0026] Furthermore, the specific process of the vulcanization treatment is as follows:

[0027] First, a flat vulcanizing machine is used to perform a first vulcanization on the mixed rubber material with the aid of a mold to obtain an intermediate rubber, and during the first vulcanization process, the temperature needs to be controlled within a range of 170° C. to 190° C., and the time is set to 3 min to 5 min;

[0028] Finally, the intermediate rubber is subjected to secondary vulcanization in a vacuum oven, and during the secondary vulcanization process, the temperature should be controlled within the range of 160° C. to 180° C., and the time is set to 1.5 h to 3 h. Finally, the secondary vulcanized intermediate rubber is placed in air and air-cooled to room temperature to obtain a unidirectional conductive rubber material.

[0029] In a third aspect, the present invention further provides an application of the above-mentioned unidirectional conductive rubber material or the unidirectional conductive rubber material prepared by the above-mentioned preparation method in the fields of electronic communications and aerospace.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The unidirectional conductive rubber material of the present invention is composed of a rubber matrix, a vulcanizing agent and modified conductive particles in a specific weight ratio. In particular, spherical conductive particles in the range of 10μm to 50μm are selected, and after surface modification, they are composite vulcanized with the rubber matrix. Because the particle size distribution of the conductive particles is uniform, the pressure is uniform during pressurized vulcanization, which avoids local non-conduction. After pressurized vulcanization, the spherical particles are deformed into an ellipsoid or a truncated cone, which increases the contact area of ​​the material in the Z-axis direction. The final product has anisotropic (Z-axis conductive, XY-axis insulating, meeting the unidirectional conductive requirements) conductive properties, high physical and mechanical properties and low density. At the same time, the periodically arranged conductive particles inside the rubber matrix have excellent electromagnetic shielding properties, and have broad application prospects in the field of unidirectional conductive requirements.

[0032] 2. In the unidirectional conductive rubber material of the present invention, the conductive filler is distributed to a specific area, which greatly increases the effective density of the conductive path, and can construct an effective conductive network with a smaller volume fraction of the conductive filler. Compared with conventional conductive rubber materials, its special distribution state is more susceptible to external stress damage, resulting in higher strain sensitivity, that is, the density of the composite material with the same electromagnetic shielding performance level is greatly reduced, meeting the characteristics of thinness and lightness.

[0033] 3. The one-way conductive rubber material provided by the present invention has improved functional groups on the surface of the conductive particles, improved the bonding between the filler and the rubber matrix, reduced the area of ​​metal directly exposed to the air, and thus delayed oxidation, thus effectively solving the problem of easy oxidation of metal fillers, significantly delaying the rate of electrical performance decay over time, and greatly improving the stability and service life of the product; at the same time, the surface-modified conductive particles have good compatibility with the rubber matrix, do not fall off, and avoid filler agglomeration and partial failure of the material. In summary, the one-way conductive rubber material of the present invention can be used for a long time and has stable performance. DETAILED DESCRIPTION

[0034] Here, exemplary embodiments will be described in detail, and the embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present invention. Instead, they are only examples consistent with some aspects of the present invention described in detail in the appended claims.

[0035] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the embodiments.

[0036] Example 1

[0037] A unidirectional conductive rubber material provided in an embodiment of the present invention comprises, by weight, 100 parts of a rubber matrix, 5 parts of a vulcanizing agent and 150 parts of modified conductive particles.

[0038] Specifically, the rubber matrix is ​​made of vinyl silicone rubber from The Dow Chemical Company of the United States.

[0039] The vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, which is from Nanjing Qiangsheng Functional Chemical Co., Ltd.

[0040] The conductive particles are spherical nickel-plated graphite particles, and the particle size of the conductive particles is 10 μm to 30 μm.

[0041] The specific steps for preparing the unidirectional conductive rubber material of this embodiment are as follows:

[0042] 1) Preparation of modified conductive particles:

[0043] Preparation of coupling agent modified liquid: Deionized water and anhydrous ethanol are measured to prepare a hydroalcohol solution, and a silane coupling agent is added to the hydroalcohol solution for hydrolysis reaction, wherein the weight ratio of deionized water, anhydrous ethanol and silane coupling agent is 8:72:20, and then stirring is continued during the process of adding acetic acid, and the pH value is adjusted to 4 to obtain a coupling agent modified liquid;

[0044] The conductive particles were modified by spraying the coupling agent modification liquid evenly on the surface of the conductive particles, wherein the weight of the silane coupling agent was 0.5% of the conductive particles, stirring at high speed and drying in a vacuum oven at 130° C. for 1 hour, and finally obtaining modified conductive particles.

[0045] 2) Preparation of unidirectional conductive rubber materials

[0046] Take 100 parts by weight of the rubber matrix, pass it through an open mill three times, then add 150 parts by weight of the modified conductive particles prepared in step 1) and 5 parts by weight of a vulcanizing agent in sequence and mix them; after standing for a period of time, perform hot pressing vulcanization to obtain a unidirectional conductive rubber material 1.

[0047] Specifically, mixing and hot pressing vulcanization are carried out according to the following process:

[0048] First, the rubber matrix, modified conductive particles, and vulcanizing agent are placed on an open mill in sequence and fully mixed until they are uniform, thereby obtaining a mixed rubber material. During the mixing process, the number of triangle packing is 12 times, and the mixing time is 40 minutes.

[0049] Then, the mixed rubber material is vulcanized for the first time by using a flat plate vulcanizer and a mold to obtain an intermediate rubber, wherein the temperature is 180° C. and the time is 4 minutes;

[0050] Finally, the intermediate rubber is subjected to secondary vulcanization in a vacuum oven at a temperature of 170° C. for 2 h. The secondary vulcanized intermediate rubber is placed in air and air-cooled to room temperature to obtain a unidirectional conductive rubber material 1 .

[0051] In order to further verify the efficacy of the unidirectional conductive rubber material 1 prepared in Example 1 of the present invention, the inventors tested its conductive properties and mechanical properties, and the test results are as follows:

[0052] According to the test standard MIL-G-83528, the shielding effectiveness of the unidirectional conductive rubber material 1 of the present embodiment 1 in the P-Ka band is measured to be 90 dB to 100 dB, and the volume resistivity in the Z-axis direction is 3×10 -3 Ω·cm, the volume resistivity in the X and Y directions is 3×10 7 Ω·cm.

[0053] According to the test standard GB / T528, the tensile strength of the unidirectional conductive rubber material 1 was measured to be 2.62 MPa, and the elongation at break was 300%.

[0054] Example 2

[0055] A unidirectional conductive rubber material provided in an embodiment of the present invention comprises, by weight, 100 parts of a rubber matrix, 3 parts of a vulcanizing agent, and 220 parts of modified conductive particles.

[0056] Specifically, the rubber matrix is ​​fluorosilicone rubber, which comes from Zhongshengjiate Materials Technology (Xi'an) Co., Ltd.

[0057] The curing agent is diisopropylbenzene oxide and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane, wherein the 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane comes from Akzo Nobel.

[0058] The conductive particles are spherical gold-nickel coated styrene particles, and the particle size of the conductive particles is 20 μm to 25 μm.

[0059] The specific steps for preparing the unidirectional conductive rubber material of this embodiment are as follows:

[0060] 1) Preparation of modified conductive particles:

[0061] Preparation of coupling agent modified liquid: Deionized water and anhydrous ethanol are measured to prepare a hydroalcohol solution, and a silane coupling agent is added to the hydroalcohol solution for hydrolysis reaction, wherein the weight ratio of deionized water, anhydrous ethanol and silane coupling agent is 7:68:25, and then stirring is continued during the process of adding acetic acid, and the pH value is adjusted to 4.5 to obtain a coupling agent modified liquid;

[0062] The conductive particles are modified by spraying the coupling agent modification liquid evenly on the surface of the conductive particles, wherein the weight of the silane coupling agent is 5% of the conductive particles, stirring at a high speed and drying in a vacuum oven at 60° C. for 3 hours, and finally obtaining modified conductive particles.

[0063] 2) Preparation of unidirectional conductive rubber materials

[0064] Take 100 parts by weight of the rubber matrix, and thin it on an open mill for 3 times. Then add 220 parts by weight of the modified conductive particles prepared in step 1) and 3 parts by weight of a vulcanizing agent in sequence and mix them. After standing for a period of time, hot-press vulcanization is performed to obtain a unidirectional conductive rubber material 2.

[0065] Specifically, mixing and hot pressing vulcanization are carried out according to the following process:

[0066] First, the rubber matrix, modified conductive particles, and vulcanizing agent are placed on an open mill in sequence and fully mixed until they are uniform, thereby obtaining a mixed rubber material. During the mixing process, the number of triangle packing is 15 times, and the mixing time is 45 minutes.

[0067] Then, the mixed rubber material is vulcanized for the first time by using a flat plate vulcanizer and a mold to obtain an intermediate rubber, during which the temperature is 190° C. and the time is 3 minutes;

[0068] Finally, the intermediate rubber is subjected to secondary vulcanization in a vacuum oven at a temperature of 160° C. for 3 hours. The secondary vulcanized intermediate rubber is placed in air and cooled to room temperature to obtain a unidirectional conductive rubber material 2.

[0069] In order to further verify the efficacy of the unidirectional conductive rubber material 2 prepared in Example 2 of the present invention, the inventors tested its conductive properties and mechanical properties, and the test results are as follows:

[0070] According to the test standard MIL-G-83528, the shielding effectiveness of the unidirectional conductive rubber material 1 of the present embodiment 1 in the P-Ka band is measured to be 90 dB to 120 dB, and the volume resistivity in the Z-axis direction is 5×10 -4 Ω·cm, the volume resistivity in the X and Y directions is 2×10 6 Ω·cm.

[0071] According to the test standard GB / T528, the tensile strength of the unidirectional conductive rubber material 1 was measured to be 2.73 MPa, and the elongation at break was 260%.

[0072] Example 3

[0073] A unidirectional conductive rubber material provided in an embodiment of the present invention comprises, by weight, 100 parts of a rubber matrix, 1 part of a vulcanizing agent and 300 parts of modified conductive particles.

[0074] Specifically, it is borosilicate rubber, which comes from Zhongshengjiate Materials Technology (Xi'an) Co., Ltd.

[0075] The curing agent is 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, which is from Akzo Nobel.

[0076] The conductive particles are spherical silver-plated aluminum particles, and the particle size of the conductive particles is 40 μm to 45 μm.

[0077] The specific steps for preparing the unidirectional conductive rubber material of this embodiment are as follows:

[0078] 1) Preparation of modified conductive particles:

[0079] Preparation of coupling agent modified liquid: Deionized water and anhydrous ethanol are measured to prepare a hydroalcohol solution, and a silane coupling agent is added to the hydroalcohol solution for hydrolysis reaction, wherein the weight ratio of deionized water, anhydrous ethanol and silane coupling agent is 5:65:30, and then stirring is continued during the process of adding acetic acid, and the pH value is adjusted to 5 to obtain a coupling agent modified liquid;

[0080] The conductive particles are modified by spraying the coupling agent modification liquid evenly on the surface of the conductive particles, wherein the weight of the silane coupling agent is 3% of the conductive particles, stirring at a high speed and drying in a vacuum oven at 110° C. for 2 hours, and finally obtaining modified conductive particles.

[0081] 2) Preparation of unidirectional conductive rubber materials

[0082] Take 100 parts by weight of the rubber matrix, pass it through an open mill three times, then add 300 parts by weight of the modified conductive particles prepared in step 1) and 1 part by weight of a vulcanizing agent in sequence and mix them; after standing for a period of time, perform hot pressing vulcanization to obtain a unidirectional conductive rubber material 3.

[0083] Specifically, mixing and hot pressing vulcanization are carried out according to the following process:

[0084] First, the rubber matrix, modified conductive particles, and vulcanizing agent are placed on an open mill in sequence and fully mixed until they are uniform, thereby obtaining a mixed rubber material. During the mixing process, the number of triangle packing is 13 times, and the mixing time is 38 minutes.

[0085] Then, the mixed rubber material is vulcanized for the first time by using a flat plate vulcanizer and a mold to obtain an intermediate rubber, wherein the temperature is 170° C. and the time is 5 minutes;

[0086] Finally, the intermediate rubber is subjected to secondary vulcanization in a vacuum oven at a temperature of 180° C. for 1.5 h. The secondary vulcanized intermediate rubber is placed in air and cooled to room temperature to obtain a unidirectional conductive rubber material 3.

[0087] In order to further verify the efficacy of the unidirectional conductive rubber material 3 prepared in Example 3 of the present invention, the inventors tested its conductive properties and mechanical properties respectively, and the test results are as follows:

[0088] According to the test standard MIL-G-83528, the shielding effectiveness of the unidirectional conductive rubber material 3 of the present embodiment 1 in the P-Ka band is measured to be 90 dB to 110 dB, and the volume resistivity in the Z-axis direction is 4×10 -4 Ω·cm, the volume resistivity in the X and Y directions is 3×10 6 Ω·cm.

[0089] According to the test standard GB / T528, the tensile strength of the unidirectional conductive rubber material 1 was measured to be 2.61 MPa, and the elongation at break was 230%.

[0090] In summary, the unidirectional conductive rubber material prepared by the present invention has the characteristic of unidirectional conductivity in the Z-axis direction. Specifically, the resistivity measured in the Z-axis direction is only 3×10 -3 Ω·cm, and the resistivity measured in the X and Y directions can reach 2×10 6 Ω·cm or more, even up to 3×10 7 Ω·cm; at the same time, it has excellent electromagnetic shielding performance, and the shielding effectiveness in the P-Ka band can reach more than 90dB, or even 120dB. In addition, the unidirectional conductive rubber material of the present invention has excellent mechanical properties, and its tensile strength can reach more than 2.6MPa, or even 2.7MPa; and its elongation at break can reach more than 230%, or even 300%.

[0091] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.

[0092] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.

Claims

1. A unidirectional conductive rubber material, characterized in that: The unidirectional conductive rubber material comprises the following raw materials by weight: 100 parts of a rubber matrix, 1 to 5 parts of a vulcanizing agent, and 150 to 300 parts of modified conductive particles; The modified conductive particles are prepared by preparing a coupling agent modification liquid or by modifying the surface of the conductive particles with a coupling agent; wherein, when preparing the coupling agent modification liquid, the coupling agent, anhydrous ethanol and deionized water are firstly mixed uniformly according to a set weight ratio, and then continuously stirred during the process of adding acetic acid, and the pH value is adjusted to 4-5, thereby completing the preparation of the coupling agent modification liquid.

2. The unidirectional conductive rubber material according to claim 1, characterized in that: When preparing the modified conductive particles, the coupling agent modification liquid or the coupling agent is evenly disposed on the surface of the conductive particles, stirred at the same time, and then dried to obtain the modified conductive particles.

3. The unidirectional conductive rubber material according to claim 1, characterized in that: When preparing the coupling agent modified liquid, the weight ratio of the coupling agent, deionized water and anhydrous ethanol is (20-30): (5-8): (65-72).

4. The unidirectional conductive rubber material according to claim 1, characterized in that: The coupling agents are all selected from silane coupling agents, and the weight ratio of the coupling agents to the conductive particles is (0.5-5):

100.

5. The unidirectional conductive rubber material according to claim 1, characterized in that: The conductive particles are any one of silver-plated copper particles, silver-plated aluminum particles, silver-plated glass particles or gold-nickel-coated styrene particles, and the particle size of the conductive particles ranges from 10 μm to 50 μm.

6. The unidirectional conductive rubber material according to claim 1, characterized in that: The rubber matrix is ​​selected from any one or more combinations of silicone rubber, fluorosilicone rubber and borosilicate rubber.

7. The unidirectional conductive rubber material according to claim 1, characterized in that: The vulcanizing agent is selected from any one or more combinations of dicumyl peroxide, dibenzoyl peroxide, and 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane.

8. A method for preparing the unidirectional conductive rubber material according to any one of claims 1 to 7, characterized in that: Firstly, the rubber matrix, the vulcanizing agent and the modified conductive particles are placed on an open mill and fully mixed until they are uniform, thereby obtaining a mixed rubber material; then, the mixed rubber material is vulcanized to obtain a unidirectional conductive rubber material.

9. The preparation method according to claim 8, characterized in that: The specific process of the vulcanization treatment is as follows: First, a flat vulcanizing machine is used to perform a first vulcanization on the mixed rubber material with the aid of a mold to obtain an intermediate rubber, and during the first vulcanization process, the temperature needs to be controlled within a range of 170° C. to 190° C., and the time is set to 3 min to 5 min; Finally, the intermediate rubber is subjected to secondary vulcanization in a vacuum oven, and during the secondary vulcanization process, the temperature should be controlled within the range of 160° C. to 180° C., and the time is set to 1.5 h to 3 h. Finally, the secondary vulcanized intermediate rubber is placed in air and air-cooled to room temperature to obtain a unidirectional conductive rubber material.