Co / Ni nanosheet wrapped double-layer shell V2O3 broadband composite absorbent and preparation method thereof

Through the preparation method of Co/Ni nanosheet wrapped double-layer shell V2O3 wide bandwidth composite absorber, the problems of insufficient absorption bandwidth and poor stability of existing microwave absorbing materials are solved, and efficient microwave absorption performance and broadband absorption bandwidth are achieved, simplifying the The process and improve the stability of the material.

CN118879276APending Publication Date: 2024-11-01XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908643.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing microwave absorbing materials have insufficient absorption bandwidth, poor stability and complex preparation processes, making it difficult to effectively solve the electromagnetic pollution problems caused by wireless electronic equipment.

Method used

The preparation method of Co/Ni nanosheet wrapped double-layer shell V2O3 wide bandwidth composite absorber is used to generate a sunflower-shaped composite absorber through hydrothermal reaction and ultrasonic treatment, thereby improving the absorption performance and absorption bandwidth.

Benefits of technology

High absorbing performance and wide absorption bandwidth are achieved, the preparation process is simplified, the stability and controllability of the material are improved, and the absorption bandwidth of the absorbing material is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879276A_ABST
    Figure CN118879276A_ABST
Patent Text Reader

Abstract

The invention discloses a Co / Ni nanosheet coated double-layer shell V2O3 broadband composite absorbent, the wave absorption range is-65.0 dB to-55 dB, and the absorption bandwidth is 2-7 GHZ. The invention further discloses the Co / Ni nanosheet wrapped double-layer shell V2O3 broadband composite absorbent, vanadium pentoxide is selected as a vanadium source, citric acid is added, and V2O3 microspheres of a double-layer shell structure are prepared through a one-step hydrothermal method. Then, cobalt nitrate hexahydrate and nickel nitrate hexahydrate are added, mixed according to a certain mass ratio and subjected to ultrasonic treatment, and the V2O3 composite wave-absorbing powder with the wide absorption bandwidth and the excellent wave-absorbing performance is prepared according to the Co / Ni and V2O3 in-situ growth principle. The method lays a foundation for development of layered composite microwave absorbing materials based on V2O3. The preparation technology has the advantages of being simple, environmentally friendly, low in cost and high in repeatability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material preparation, and specifically relates to a Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorbent, and also relates to a preparation method of the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorbent. Background Art

[0002] The iterative updates and growing demand for wireless electronic devices have led to an incremental increase in electromagnetic pollution, which not only has a negative impact on high-tech devices but also poses a threat to human health. In order to address this problem, it is necessary to research and develop new materials with effective microwave absorption properties.

[0003] In recent years, Co-based and Ni-based metal oxides with dual loss characteristics are becoming the preferred materials for research. Among them, metal Co and Ni have the advantages of high saturation magnetization and high conductivity. V2O3 is considered to be a potential microwave absorbing material due to its superior dielectric loss. Although V2O3 absorbers with specific morphologies have good absorption properties, the insufficient absorption bandwidth of a single material, the poor stability of the composite material, and the complex preparation process are still difficult problems that need to be solved urgently. Summary of the invention

[0004] The invention aims to provide a Co / Ni nanosheet-wrapped double-shell V2O3 wide-bandwidth composite absorber, which has high wave absorbing performance and absorption bandwidth.

[0005] Another object of the present invention is to provide a method for preparing a Co / Ni nanosheet-wrapped double-shell V2O3 wide-bandwidth composite absorber, which can accurately control the morphology and structure of the material to generate a sunflower-shaped composite absorbing material, which not only increases the absorption bandwidth of the absorbing material, but also significantly improves the absorbing performance.

[0006] The first technical solution adopted by the present invention is that Co / Ni nanosheets wrap double-shell V2O3 wide-bandwidth composite absorber, the absorption wave range is -65.0dB to -55dB, and the absorption bandwidth is 2-7GHZ.

[0007] The second technical solution adopted by the present invention is a method for preparing a Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber, which is specifically implemented according to the following steps:

[0008] Step 1, dissolving citric acid and V2O5 in deionized water at 60-90°C, uniformly mixing by ultrasonication for 10-60 minutes to obtain a mixed solution 1, transferring the mixed solution 1 to a hydrothermal reactor, and cooling to room temperature; collecting the precipitate and placing it in a vacuum tube furnace for annealing at a heating temperature of 450-550°C for 2-4 hours to obtain double-shell V2O3 microspheres;

[0009] Step 2, dissolving cobalt nitrate hexahydrate and nickel nitrate hexahydrate in ethylene glycol to prepare a mixed aqueous solution 2, and ultrasonicating for 10-60 minutes to obtain a Co / Ni mixed aqueous solution;

[0010] Step 3, add double-shell V2O3 microsphere powder to Co / Ni mixed aqueous solution, ultrasonicate for 30-90 minutes, and obtain mixed solution 3; transfer mixed solution 3 to a reactor, and after cooling to room temperature, collect the precipitate and place it in a vacuum tube furnace for annealing at a heating temperature of 650-750°C for 1-3 hours to obtain sunflower-shaped Co / Ni / V2O3 microspheres, that is, Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorbent.

[0011] The present invention is also characterized in that:

[0012] In step 1, the mass ratio of V2O5 to citric acid is 1:2-4, and the volume ratio of citric acid to deionized water is 1:2.

[0013] In step 1, the mixed solution 1 is transferred to a hydrothermal reactor at a drying temperature of 190-210° C. and a drying time of 15-25 h.

[0014] In step 1, the precipitate is placed in a vacuum tube furnace and heated at a temperature of 450-550° C. for 2-4 hours under an argon atmosphere.

[0015] In step 2, the mass ratio of cobalt nitrate hexahydrate to nickel nitrate hexahydrate is 1:1, and the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 1-250 g.

[0016] In step 3, the mass ratio of the double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:0.5-2.5.

[0017] In step 3, the mixed solution 3 is transferred to a reaction kettle and set to: a drying temperature of 150-180° C. and a drying time of 10-16 h.

[0018] After annealing in the vacuum tube furnace in step 3, the heating temperature is 650-750° C. and the heating time is 1-3 h under argon atmosphere.

[0019] The beneficial effects of the present invention are:

[0020] The Co / Ni nanosheet-wrapped double-shell V2O3 wide-bandwidth composite absorber of the present invention is in the shape of a sunflower and has high wave-absorbing performance and a wide absorption bandwidth.

[0021] The preparation method of the Co / Ni nanosheet-wrapped double-shell V2O3 wide-bandwidth composite absorber of the present invention is simpler and easier to implement than the traditional method, and the operation steps are simple and easy to control. The morphology and structure of the material can be accurately controlled to generate a sunflower-shaped composite absorbing material, which not only increases the absorption bandwidth of the absorbing material, but also significantly improves the absorbing performance. The method has stable process and strong controllability, and can ensure that the prepared composite absorbing material has good repeatability and consistency. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope image of the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber obtained in Example 2;

[0023] Figure 2 is a cross-sectional scanning electron microscope image of the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber obtained in Example 5;

[0024] Figure 3 is a scanning electron microscope image of the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber obtained in Example 6;

[0025] Figure 4 This is an absorption bandwidth efficiency diagram of the samples at different mass ratios of double-layer shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate in the embodiments. DETAILED DESCRIPTION

[0026] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0027] Co / Ni nanosheets wrapped double-shell V2O3 wide bandwidth composite absorber, the absorption wave range is -65.0dB ~ -55dB, the absorption bandwidth is 2-7GHZ.

[0028] The preparation method of the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber is specifically implemented according to the following steps:

[0029] Step 1, dissolving citric acid and V2O5 in deionized water at 60-90°C, uniformly mixing by ultrasonication for 10-60 minutes to obtain a mixed solution 1, transferring the mixed solution 1 to a hydrothermal reactor, and cooling to room temperature; collecting the precipitate and placing it in a vacuum tube furnace for annealing at a heating temperature of 450-550°C for 2-4 hours to obtain double-shell V2O3 microspheres;

[0030] The mass ratio of V2O5 to citric acid is 1:2-4, and the volume ratio of citric acid to deionized water is 1:2.

[0031] The mixed solution 1 is transferred to a hydrothermal reactor and dried at a temperature of 190-210°C for 15-25 hours.

[0032] After placing the precipitate in a vacuum tube furnace, the heating temperature is 450-550°C and the heating time is 2-4h under argon atmosphere.

[0033] Step 2, dissolving cobalt nitrate hexahydrate and nickel nitrate hexahydrate in ethylene glycol to prepare a mixed aqueous solution 2, and ultrasonicating for 10-60 minutes to obtain a Co / Ni mixed aqueous solution;

[0034] The mass ratio of cobalt nitrate hexahydrate to nickel nitrate hexahydrate is 1:1, and the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1ml:1-250g.

[0035] Step 3, add double-shell V2O3 microsphere powder to Co / Ni mixed aqueous solution, ultrasonicate for 30-90 minutes, and obtain mixed solution 3; transfer mixed solution 3 to a reactor, and after cooling to room temperature, collect the precipitate and place it in a vacuum tube furnace for annealing at a heating temperature of 650-750°C for 1-3 hours to obtain sunflower-shaped Co / Ni / V2O3 microspheres, that is, Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorbent.

[0036] The mass ratio of the double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:0.5-2.5.

[0037] The mixed solution 3 was transferred to a reaction kettle and set to: drying temperature of 150-180°C, drying time of 10-16h.

[0038] After annealing in a vacuum tube furnace, the heating temperature is 650-750°C and the heating time is 1-3h under argon atmosphere.

[0039] Example 1

[0040] Under ultrasound at 80°C, V2O5 and citric acid were dissolved in 40 mL of deionized water in a mass ratio of 1:3 to obtain a black-blue mixed solution 1, and ultrasound was continued for 50 min. The obtained mixed solution 1 was transferred to a hydrothermal reactor (304 stainless steel / 50 ml high temperature resistant reactor) and reacted at 200°C for 20 h. The precipitate was collected and placed in a vacuum tube furnace. Under argon atmosphere, the heating rate was 5°C / min to 500°C, and the heating time was 3 h to obtain a double-shell V2O3 microsphere powder.

[0041] A mixed aqueous solution 2 of cobalt nitrate hexahydrate and nickel nitrate hexahydrate with ethylene glycol solution in a mass ratio of 1:1, wherein the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 250 g. Ultrasonic treatment is performed at room temperature (ultrasonic power is 120 w) for 30 minutes to obtain a Co / Ni mixed aqueous solution.

[0042] Take double-shell V2O3 microsphere powder and add it to the Co / Ni mixed aqueous solution, where the mass ratio of double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:2.5. Then transfer the mixture to a 100mL high-temperature resistant reactor, keep it at 150℃ for 12h, and wait until it cools to room temperature. Collect the precipitate and place it in a vacuum tube furnace for annealing. Under argon atmosphere, the heating rate is 3℃ / min to 700℃ for 2h, and then a sunflower-shaped Co / Ni / V2O3 composite absorbent is obtained.

[0043] Example 2

[0044] Under ultrasound at 80°C, V2O5 and citric acid were dissolved in 40 mL of deionized water in a mass ratio of 1:3 to obtain a black-blue mixed solution 1, and ultrasound was continued for 50 min. The obtained mixed solution 1 was transferred to a hydrothermal reactor (304 stainless steel / 50 ml high temperature reactor) and reacted at 200°C for 20 h. The precipitate was collected and placed in a vacuum tube furnace. Under argon atmosphere, the heating rate was 7°C / min to 500°C for 3 h to obtain a double-shell V2O3 microsphere powder.

[0045] A mixed aqueous solution 2 of cobalt nitrate hexahydrate and nickel nitrate hexahydrate with ethylene glycol solution in a mass ratio of 1:1, wherein the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 250 g. Ultrasonic treatment is performed at room temperature (ultrasonic power is 120 w) for 30 minutes to obtain a Co / Ni mixed aqueous solution.

[0046] Take double-shell V2O3 microsphere powder and add it to the Co / Ni mixed aqueous solution, where the mass ratio of double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:2.5. Then transfer the mixture to a 100mL high-temperature resistant reactor, keep it at 160℃ for 12h, and cool it to room temperature. Collect the precipitate and place it in a vacuum tube furnace for annealing. Under argon atmosphere, the heating rate is 4℃ / min to 700℃ for 2h, and then Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorbent is obtained. Figure 1 This is a scanning electron microscope image of the sunflower-shaped Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber obtained in Example 2. Figure 1It can be seen that a small amount of Co / Ni / nanosheets can be clearly observed distributed on the surface of the double-shell V2O3 microspheres.

[0047] Example 3

[0048] Under ultrasound at 80°C, V2O5 and citric acid were dissolved in 40 mL of deionized water in a mass ratio of 1:3 to obtain a black-blue mixed solution 1, and ultrasound was continued for 50 min. The obtained mixed solution 1 was transferred to a hydrothermal reactor (304 stainless steel / 50 ml high temperature resistant reactor) and reacted at 200°C for 20 h. The precipitate was collected and placed in a vacuum tube furnace. Under argon atmosphere, the heating rate was 5-10°C / min to 500°C for 3 h to obtain a double-shell V2O3 microsphere powder.

[0049] A mixed aqueous solution 2 of cobalt nitrate hexahydrate and nickel nitrate hexahydrate with ethylene glycol solution in a mass ratio of 1:1, wherein the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 250 g. Ultrasonic treatment is performed at room temperature (ultrasonic power is 120 w) for 30 minutes to obtain a Co / Ni mixed aqueous solution.

[0050] Take double-shell V2O3 microsphere powder and add it to the Co / Ni mixed aqueous solution, where the mass ratio of double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:2.5. Then transfer the mixture to a 100mL high-temperature resistant reactor, keep it at 170℃ for 12h, and wait until it cools to room temperature. Collect the precipitate and place it in a vacuum tube furnace for annealing. Under argon atmosphere, the heating rate is 5℃ / min to 700℃ for 2h, and then Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorbent is obtained.

[0051] Example 4

[0052] Under ultrasound at 80°C, V2O5 and citric acid were dissolved in 40 mL of deionized water in a mass ratio of 1:3 to obtain a black-blue mixed solution 1, and ultrasound was continued for 50 min. The obtained mixed solution 1 was transferred to a hydrothermal reactor (304 stainless steel / 50 ml high temperature resistant reactor) and reacted at 200°C for 20 h. The precipitate was collected and placed in a vacuum tube furnace. Under argon atmosphere, the heating rate was 5-10°C / min to 500°C for 3 h to obtain a double-shell V2O3 microsphere powder.

[0053] A mixed aqueous solution 2 of cobalt nitrate hexahydrate and nickel nitrate hexahydrate with ethylene glycol solution in a mass ratio of 1:1, wherein the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 250 g. Ultrasonic treatment is performed at room temperature (ultrasonic power is 120 w) for 30 minutes to obtain a Co / Ni mixed aqueous solution.

[0054] Take double-shell V2O3 microsphere powder and add it to the Co / Ni mixed aqueous solution, where the mass ratio of double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:2.5. Then transfer the mixture to a 100mL high-temperature resistant reactor, keep it at 180℃ for 12h, and wait until it cools to room temperature. Collect the precipitate and place it in a vacuum tube furnace for annealing. Under argon atmosphere, the heating rate is 2℃ / min to 700℃ for 2h, and then a sunflower-shaped Co / Ni / V2O3 composite absorbent is obtained.

[0055] Example 5

[0056] Under ultrasound at 80°C, V2O5 and citric acid were dissolved in 40 mL of deionized water in a mass ratio of 1:3 to obtain a black-blue mixed solution 1, and ultrasound was continued for 50 min. The obtained mixed solution 1 was transferred to a hydrothermal reactor (304 stainless steel / 50 ml high temperature resistant reactor) and reacted at 200°C for 20 h. The precipitate was collected and placed in a vacuum tube furnace. Under argon atmosphere, the heating rate was 5-10°C / min to 500°C for 3 h to obtain a double-shell V2O3 microsphere powder.

[0057] A mixed aqueous solution 2 of cobalt nitrate hexahydrate and nickel nitrate hexahydrate in a mass ratio of 1:1 and ethylene glycol solution, wherein the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 100 g, is placed at room temperature for ultrasonic treatment (ultrasonic power is 120w), and the ultrasonic time is continued for 30 minutes to obtain a Co / Ni mixed aqueous solution.

[0058] Take double-shell V2O3 microsphere powder and add it to the Co / Ni mixed aqueous solution, where the mass ratio of double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:1. Then transfer the mixture to a 100mL high-temperature resistant reactor, keep it at 160℃ for 12h, and wait until it cools to room temperature. Collect the precipitate and place it in a vacuum tube furnace for annealing. Under argon atmosphere, the heating rate is 3℃ / min to 700℃ for 2h, and then obtain Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorber. The absorption intensity of the obtained composite absorber reaches -60.0dB. Figure 2 This is a cross-sectional scanning electron microscope image of the sunflower-shaped Co / Ni / V2O3 composite absorbent obtained in Example 5. Figure 2 It can be seen that the composite absorbent prepared in Example 6 with a mass of 0.25 g of cobalt nitrate hexahydrate and nickel nitrate hexahydrate (mass ratio 1:1) has the best morphology. The surface of V2O3 is evenly wrapped by Co / Ni nanosheets, and a double-layer shell structure is observed inside the V2O3 microspheres at the opening.

[0059] Example 6

[0060] Under ultrasound at 80°C, V2O5 and citric acid were dissolved in 40 mL of deionized water in a mass ratio of 1:3 to obtain a black-blue mixed solution 1, and ultrasound was continued for 50 min. The obtained mixed solution 1 was transferred to a hydrothermal reactor (304 stainless steel / 50 ml high temperature resistant reactor) and reacted at 200°C for 20 h. The precipitate was collected and placed in a vacuum tube furnace. Under argon atmosphere, the heating rate was 5-10°C / min to 500°C for 3 h to obtain a double-shell V2O3 microsphere powder.

[0061] A mixed aqueous solution 2 of cobalt nitrate hexahydrate and nickel nitrate hexahydrate in a mass ratio of 1:1 and ethylene glycol solution, wherein the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:1, is placed at room temperature for ultrasonic treatment (ultrasonic power is 120w), and the ultrasonic time is continued for 30min to obtain a Co / Ni mixed aqueous solution.

[0062] Take double-shell V2O3 microsphere powder and add it to the Co / Ni mixed aqueous solution, where the mass ratio of double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1:0.5. Then transfer the mixture to a 100mL high-temperature resistant reactor, keep it at 160℃ for 12h, and wait until it cools to room temperature. Collect the precipitate and place it in a vacuum tube furnace for annealing. Under argon atmosphere, the heating rate is 2-5℃ / min to 700℃ for 2h, and then obtain Co / Ni nanosheets wrapped double-shell V2O3 wide-bandwidth composite absorber. The effective absorption bandwidth of the obtained composite absorber reaches 6.82GHz. Figure 3 This is a scanning electron microscope image of the sunflower-shaped Co / Ni / V2O3 composite absorber obtained in Example 6. Figure 3 It can be seen that it can be clearly observed that the Co / Ni nanosheets completely wrap the V2O3 microspheres, and the Co / Ni nanosheets present a typical nanoflower shape.

[0063] According to Examples 1-4 of the present invention, composite absorbers were obtained under different experimental environments with a system ratio of 1 ml:250 g for ethylene glycol and a mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate. After experimental comparison, the experimental conditions of Example 2 are preferred. Examples 5-6 are composite absorbers with different mass ratios of double-layer shell V2O3 microsphere powder and a mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate under the same experimental environment, which are 1:1 and 1:0.5 respectively. By adjusting the mass ratio of V2O3 microsphere powder and the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate, the heterogeneous interface and dipole polarization degree of the composite absorber can be effectively regulated to regulate the wave absorption intensity and absorption bandwidth performance. The widest absorption bandwidth of the Co / Ni / V2O3 composite absorber obtained by the present invention is 6.82 GHz, which is 64.8% higher than that of pure V2O3. Figure 4 As shown, the composite absorber with a mass ratio of double-shell V2O3 microsphere powder to a mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate of 1:0.5 has an absorption bandwidth of 6.82GHz; the composite absorber with a mass ratio of double-shell V2O3 microsphere powder to a mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate of 1:1 has a microwave absorption performance of -60.0dB. It can be concluded that the obtained Co / Ni / V2O3 composite absorber has high absorption performance and broadband absorption bandwidth.

[0064] Through the above method, the present invention provides a method for preparing a sunflower-shaped Co / Ni nanosheet-wrapped double-shell V2O3 wide-bandwidth composite absorber, which has a simple preparation process, is easy to control, and has a low production cost; the Co / Ni / V2O3 composite absorber has excellent microwave absorption performance and a wide absorption bandwidth. The film provides more possibilities for the preparation of V2O3-based films.

Claims

1. Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorber, characterized in that: The absorption wave range is -65.0dB ~ -55dB, and the absorption bandwidth is 2-7GHZ.

2. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 1, characterized in that: Follow the steps below to implement it: Step 1, dissolving citric acid and V2O5 in deionized water at 60-90°C, uniformly mixing by ultrasonication for 10-60 minutes to obtain a mixed solution 1, transferring the mixed solution 1 to a hydrothermal reactor, and cooling to room temperature; collecting the precipitate and placing it in a vacuum tube furnace for annealing at a heating temperature of 450-550°C for 2-4 hours to obtain double-shell V2O3 microspheres; Step 2, dissolving cobalt nitrate hexahydrate and nickel nitrate hexahydrate in ethylene glycol to prepare a mixed aqueous solution 2, and ultrasonicating for 10-60 minutes to obtain a Co / Ni mixed aqueous solution; Step 3, add double-shell V2O3 microsphere powder to Co / Ni mixed aqueous solution, ultrasonicate for 30-90 minutes, and obtain mixed solution 3; transfer mixed solution 3 to a reactor, and after cooling to room temperature, collect the precipitate and place it in a vacuum tube furnace for annealing at a heating temperature of 650-750°C for 1-3 hours to obtain sunflower-shaped Co / Ni / V2O3 microspheres, that is, Co / Ni nanosheets wrapped double-shell V2O3 broadband composite absorbent.

3. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 2, characterized in that: In step 1, the mass ratio of V2O5 to citric acid is 1:2-4, and the volume ratio of citric acid to deionized water is 1:

2.

4. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 2, characterized in that: In step 1, the mixed solution 1 is transferred to a hydrothermal reactor and the drying temperature is 190-210° C. and the drying time is 15-25 h.

5. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 2, characterized in that: In step 1, the precipitate is placed in a vacuum tube furnace and heated at a temperature of 450-550° C. for 2-4 hours under an argon atmosphere.

6. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 2, characterized in that: The mass ratio of cobalt nitrate hexahydrate to nickel nitrate hexahydrate in step 2 is 1:1, and the mass ratio of ethylene glycol to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate is 1 ml: 1-250 g.

7. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 2, characterized in that: The mass ratio of the double-shell V2O3 microsphere powder to the mixture of cobalt nitrate hexahydrate and nickel nitrate hexahydrate in step 3 is 1:0.5-2.

5.

8. The method for preparing the Co / Ni nanosheet-wrapped double-shell V2O3 broadband composite absorber according to claim 2, characterized in that: In step 3, the mixed solution 3 is transferred to a reaction kettle and set to: a drying temperature of 150-180° C. and a drying time of 10-16 h.