Purifying agent as well as preparation method and application thereof

By controlling the proportion of pore structure and pore-making agent in the dechlorination agent, a large-pore-small-medium pore structure is formed, the problem of low chlorine capacity of the existing dechlorination agent is solved, and the passage of gas and liquid phase dechlorination agents is improved The chlorine permeable capacity and maintain mechanical strength, meeting the dechlorination needs of the reforming device.

CN118879360APending Publication Date: 2024-11-01CHINA NAT OFFSHORE OIL CORP +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411017686.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing dechlorination agents are low in the petroleum refining industry, especially in the liquid phase dechlorination process. Due to the existence of water, the dechlorination agent structure damage and mass transfer resistance are large, resulting in insufficient chlorination capacity and cannot meet the reforming. Dechlorination requirements for the device.

Method used

By controlling the distribution of pore structures in the inner and outer layers of the purifier, the inner layer is small and medium-sized pores of 10-50nm and the outer layer is pores greater than 50nm. Combined with the proportional regulation of the pore-forming agent, a large-pore-small and medium-sized pore structure is formed to improve the reaction gas The penetration and mechanical strength overcome the resistance of liquid mass transfer and improve penetration of chlorine capacity.

Benefits of technology

The chlorine capacity of the gas-phase dechlorination agent reaches more than 50%, the penetrating chlorine capacity of the liquid-phase dechlorination agent reaches more than 25%, and maintains a high crushing strength, meets the dechlorination requirements of the continuous reforming device, and has good desulfurization effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967496410000121
    Figure BDA0004967496410000121
Patent Text Reader

Abstract

The invention relates to the technical field of dechlorination, in particular to a purifying agent as well as a preparation method and application thereof. The purifying agent comprises an inner core and a shell at least partially wrapping the outer surface of the inner core, and in the inner core, the proportion of the pore volume with the pore diameter being 10-50 nm to the total pore volume is larger than or equal to 64%; in the shell, the proportion of the pore volume with the pore diameter larger than 50 nm to the total pore volume is larger than or equal to 24%. The preparation method comprises the following steps: mixing and granulating the raw materials of the inner core in proportion to obtain the inner core, mixing the raw materials of the shell, coating the outer surface of the inner core with the mixed raw materials of the shell, and drying and roasting to obtain the catalyst, in the raw materials of the inner core, the percentage of the pore-forming agent in the total mass of the active component and the carrier is A; in the raw materials of the shell, the percentage of the pore-forming agent in the total mass of the active component and the carrier is B; 3% < = A < = 6%, 6% < = B < = 18%, and A: B = 1: 2-6. The prepared purifying agent is high in chlorine capacity, and meets the gas-phase and liquid-phase dechlorination requirements of a continuous reforming device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of dechlorination, and in particular to a purifying agent and a preparation method and application thereof. Background Art

[0002] In the petroleum refining industry, with the continuous development of catalytic reforming technology and the continuous improvement of the processing capacity of the reforming unit, the amount of hydrogen chloride produced in this section has gradually increased. A large amount of organic chloride reacts to generate hydrogen chloride and combines with water in the system to generate highly corrosive hydrochloric acid, which will corrode the equipment and have a serious impact on normal production. Therefore, it is very necessary to remove hydrogen chloride. At present, the dechlorination effect of the dechlorination agent for removing chlorine-containing gas in the reforming unit is still unsatisfactory in use. The chlorine capacity of the gas phase dechlorination agent in the market is less than 40%, and the chlorine capacity of the liquid phase dechlorination agent is less than 20%. For the liquid phase dechlorination of reforming oil, the operating temperature is relatively low, generally not exceeding 70°C. The reforming oil contains a small amount of water, and water has a greater impact on the dechlorination agent with alkali metal as the active component. This is because under the conditions of liquid phase dechlorination, water will react with the dechlorinated substances such as calcium chloride and magnesium chloride, causing the dechlorination agent structure to be destroyed and the internal pores to be blocked. On the other hand, the liquid phase mass transfer resistance of the reforming oil is relatively large. These unfavorable factors ultimately lead to a decrease in chlorine capacity.

[0003] The active components of domestic blending dechlorination agents are mostly oxides, hydroxides and carbonates of alkali metals and alkaline earth metals such as Na2CO3, NaOH, NaHCO3, CaO, CaCO3, and some products use organic amines as active components. At the same time, the carriers are mostly cheap and readily available porous substances such as alumina, diatomaceous earth, and kaolin, and organic and polymer additives are added. Dechlorination agent products are made through mixing, molding, drying, and roasting.

[0004] CN101773768A discloses a dry dechlorinating agent for removing HCl from gas and its preparation method. The dechlorinating agent uses Na2CO3, CaCO3, CaO, and MgO as active components, cross-linked bentonite as a porosity aid, and methyl cellulose as a foaming agent and an extrusion aid. It is formed into strips, and then dried and roasted to make a dechlorinating agent. Cross-linked bentonite uses larger polyaluminum cations to exchange smaller simple cations, so the pore system is well-developed and the specific surface area is large. The specific surface area and pore volume of cross-linked bentonite are larger than those of non-cross-linked bentonite. Using cross-linked bentonite as a porosity aid for the dechlorinating agent increases the specific surface area of ​​the dechlorinating agent, and increases the dechlorination activity and chlorine capacity of the dechlorinating agent. The pore volume of the dechlorinating agent made of cross-linked bentonite is 0.3mL / g-0.4mL / g, and the specific surface area is 70m 2 / g-90m 2 / g, the crushing strength is 60N / cm-80N / cm, the chlorine capacity is 12.3%~20.1%, and the chlorine capacity still needs to be improved.

[0005] CN1724119A discloses a method for preparing a dechlorinating agent, wherein polyhexenol, bentonite and alkyl ammonium salt are subjected to a slurry synthesis reaction with an aqueous solution containing sodium hydroxide, magnesium hydroxide and copper hydroxide at 40-80°C, and after the reaction is completed, the reaction product is extruded and formed, dried at 80-100°C for 4 hours, and then roasted at 650°C for 10 hours to obtain the dechlorinating agent. Although the dechlorinating agent in the above technology is molten at 823K, 0.1mg / m 3 The chlorine penetration capacity of chlorine is 55.3%, but its chlorine penetration capacity at room temperature is very small, less than 20%.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The first purpose of the present invention is to provide a dechlorination purifier, which improves the chlorine capacity of the purifier by controlling the different distribution of the pore structure of the inner and outer layers of the purifier, meets the gas and liquid phase dechlorination requirements of the continuous reforming device, and solves the problem of low chlorine capacity of the existing dechlorination agent.

[0008] The second object of the present invention is to provide a method for preparing the dechlorination purifier as described above. When preparing the purifier, the method of the present invention controls the content of the pore-forming agent in the inner layer raw material and the outer layer raw material of the purifier, so that the purifier presents a macropore-medium and small pore structure from the outside to the inside, which is conducive to the penetration of the reaction gas, and can overcome the difficulty of the large liquid phase mass transfer resistance of the reformed oil, improve the penetration chlorine capacity, and at the same time maintain a high crushing strength.

[0009] The third object of the present invention is to use the dechlorination purifier as described above in a reforming gas phase and liquid phase dechlorination process or a fuel gas desulfurization process.

[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0011] A purifier comprises a core and a shell at least partially covering the outer surface of the core, wherein the pore volume with a pore size of 10-50 nm in the core accounts for ≥64% of the total pore volume; and the pore volume with a pore size of more than 50 nm in the shell accounts for ≥24% of the total pore volume.

[0012] A method for preparing the purifier as described above comprises the following steps:

[0013] The raw materials of the inner core are mixed and granulated according to a proportion to obtain the inner core, the raw materials of the outer shell are mixed and coated on the outer surface of the inner core, and the purifier is obtained by drying and roasting;

[0014] In the raw materials of the inner core, the percentage of the pore-forming agent in the total mass of the active components and the carrier is A; in the raw materials of the outer shell, the percentage of the pore-forming agent in the total mass of the active components and the carrier is B; and the following conditions are satisfied: 3%≤A≤6%, 6%≤B≤18%, A:B=1:2-6.

[0015] An application of the purifier as described above in a reforming gas phase and liquid phase dechlorination process or a fuel gas desulfurization process.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] (1) The dechlorination purifier provided by the present invention has the advantages of high chlorine capacity and wide raw material adaptability, and meets the gas phase and liquid phase dechlorination requirements of the continuous reforming device. The gas phase penetration chlorine capacity can reach more than 50%, the liquid phase penetration chlorine capacity can reach more than 25%, and it also has a good desulfurization effect.

[0018] (2) The preparation process of the method of the present invention is simple, and the prepared purifier has the advantages of high mechanical strength and long service life. The method of the present invention adjusts the pore distribution of the purifier by controlling the content and proportion of the pore-forming agent in the inner and outer layer mixtures, thereby forming a pore structure in which large pores of 50 nm or more are concentrated in the outer layer of the purifier and small and medium pores of 10-50 nm are concentrated in the inner layer. While maintaining a high crushing strength, it is conducive to the penetration of the reaction gas, and can overcome the difficulty of large liquid phase mass transfer resistance of the reformed oil, thereby improving the penetration chlorine capacity. DETAILED DESCRIPTION

[0019] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0020] A first aspect of the present invention provides a purifier, comprising a core and a shell at least partially covering the outer surface of the core, wherein the core has a pore volume with a pore size of 10-50 nm accounting for ≥64% of the total pore volume; for example, 64.17%, 65.49%, 77.14%, 77.35%, 78.17%, 78.69%, 79.31%, etc.; in the shell, the pore volume with a pore size of >50 nm accounts for ≥24% of the total pore volume, for example, 24.21%, 44.28%, 47.21%, 50.23%, 60.25%, 61.11%, 63.94%, etc.

[0021] The present invention controls the pore distribution of the inner layer and the outer layer of the purifier, and makes the pore structure conducive to the penetration of the reaction gas while maintaining a high crushing strength, and can overcome the difficulty of large liquid phase mass transfer resistance of the reformed oil, thereby improving the penetration chlorine capacity. The purifier provided by the present invention has a gas phase penetration chlorine capacity of up to 50% and a liquid phase penetration chlorine capacity of up to 25%. It has the advantages of high chlorine capacity and wide raw material applicability, meets the gas phase and liquid phase dechlorination requirements of the continuous reforming device, and also has a good desulfurization effect.

[0022] In some preferred embodiments of the present invention, the percentage of pore volume with pore diameter greater than 50 nm in the shell is ≥ 44% of the total pore volume, so that the purifier forms a pore structure with concentrated distribution of large pores (greater than 50 nm) in the outer layer and concentrated distribution of small pores (10-50 nm) in the inner layer, which can ensure a high crushing strength, facilitate the infiltration of reaction gas, and reduce the liquid phase mass transfer resistance.

[0023] In some specific embodiments of the present invention, the diameter of the inner core is 1-5 mm, such as 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, etc., and the thickness of the outer shell accounts for 1 / 4-1 / 2 of the radius of the purifier, such as 1 / 4, 1 / 3, 1 / 2, etc.

[0024] In some specific embodiments of the present invention, the raw materials of the core and the shell both include active components, carriers and pore-forming agents.

[0025] In some specific embodiments of the present invention, the active component includes an alkaline earth metal compound and / or a transition metal oxide.

[0026] In some specific embodiments of the present invention, the alkaline earth metal compound includes at least one of a salt, an oxide or a hydroxide of an alkaline earth metal.

[0027] In some specific embodiments of the present invention, the transition metal oxide includes at least one of zinc oxide, copper oxide and iron oxide.

[0028] In some specific embodiments of the present invention, the carrier includes at least one of alumina, molecular sieves and minerals.

[0029] In some specific embodiments of the present invention, the alumina includes pseudo-boehmite, and preferably has a powdery structure. Pseudo-boehmite is also known as monohydrated alumina, pseudo-boehmite, with a chemical formula of AlOOH·nH2O, n=0.08-0.62, good peptization performance, strong adhesion, high specific surface area, large pore volume and the like. Its water-containing state is a thixotropic gel. Its application in the present invention can obtain a dechlorination agent with a better pore structure.

[0030] In some specific embodiments of the present invention, the molecular sieve includes X-type molecular sieve and / or Y-type molecular sieve.

[0031] In some specific embodiments of the present invention, the mineral comprises at least one of kaolin, sepiolite and clay, and the mineral is preferably in a powdery structure.

[0032] In some specific embodiments of the present invention, the pore-forming agent includes methylcellulose and / or sesbania. The pore-forming agent plays a role in adjusting or controlling the pore structure of the product. Under high-temperature roasting conditions, the pore-forming agent will burn or volatilize, leaving pores, which form pores in the purifier, thereby preparing a porous purifier structure, achieving efficient removal of chlorine-containing and sulfur-containing media and structural stability.

[0033] A second aspect of the present invention provides a method for preparing the purifier as described above, comprising the following steps:

[0034] The raw materials of the inner core are mixed and granulated according to a proportion to obtain the inner core, the raw materials of the outer shell are mixed and coated on the outer surface of the inner core, and the purifier is obtained by drying and roasting;

[0035] In the raw materials of the inner core, the percentage of the pore-forming agent in the total mass of the active components and the carrier is A; in the raw materials of the outer shell, the percentage of the pore-forming agent in the total mass of the active components and the carrier is B; and the following conditions are satisfied: 3%≤A≤6%, 6%≤B≤18%, A:B=1:2-6.

[0036] The method of the present invention controls the content of the pore-forming agent in the raw materials of the inner and outer layers so that the percentage content A of the pore-forming agent in the raw materials of the inner layer is less than the percentage content B of the pore-forming agent in the raw materials of the outer layer, and the ratio thereof is controlled between 1:2-6, so as to facilitate the formation of a small and medium-sized pore structure in the inner layer and a large pore structure in the outer layer, so that the prepared purifier has large pores (greater than 50 nm) distributed in a concentrated manner in the outer layer and small and medium-sized pores (10-50 nm) distributed in a concentrated manner in the inner layer, forming a pore structure characteristic of large pores-small and medium-sized pores from the outside to the inside, achieving better strength and maintaining a good pore structure, so as to facilitate the penetration of reaction gas, reduce liquid phase mass transfer resistance, and increase penetration chlorine capacity.

[0037] For example, in different embodiments, A can be any point value among 3%, 4%, 5%, 6%, or a range value consisting of any two point values; B can be any point value among 6%, 9%, 12%, 15%, 18%, or a range value consisting of any two point values; A:B can be any point value among 1:2, 1:3, 1:4, 1:5, 1:6, or a range value consisting of any two point values.

[0038] In some specific embodiments of the present invention, the granulation method of the kernel is rotary granulation, comprising the following steps: mixing the raw materials of the kernel and placing them in a granulator, spraying nitric acid solution and water in a rotary state for granulation to obtain the kernel.

[0039] In some specific embodiments of the present invention, the raw material of the shell is coated on the outer surface of the inner core by a rotational granulation method, comprising the following steps: mixing the raw materials of the shell and placing them in a granulator, placing the inner core into the mixture of the shell, and spraying nitric acid solution and water in a rotating state for granulation.

[0040] In some specific embodiments of the present invention, the granulator is a disc granulator.

[0041] In some specific embodiments of the present invention, when the kernel is granulated, the rotation speed of the granulator is 10-20r / min, for example, any point value among 10r / min, 12r / min, 14r / min, 16r / min, 18r / min, 20r / min, or a range value consisting of any two point values, and the granulation time is 0.5-5h, for example, any point value among 0.5h, 1h, 2h, 3h, 4h, 5h, or a range value consisting of any two point values.

[0042] In some specific embodiments of the present invention, when coating the raw material of the shell, after spraying the nitric acid solution and water, the granulator first operates at a speed of 20-30r / min for 1-10min, for example, the speed of the granulator can be any point value among 20r / min, 22r / min, 24r / min, 26r / min, 28r / min, 30r / min or a range value composed of any two point values, the rotation time can be any point value among 1min, 3min, 5min, 8min, 10min or a range value composed of any two point values, and then granulation is carried out at a speed of 10-20r / min, for example, any point value among 10r / min, 12r / min, 14r / min, 16r / min, 18r / min, 20r / min or a range value composed of any two point values, and the granulation time is 0.5-5h, for example, any point value among 0.5h, 1h, 2h, 3h, 4h, 5h or a range value composed of any two point values.

[0043] When coating the shell raw material onto the outer surface of the inner core, first rotating at high speed for a period of time helps the materials to be mixed more evenly, forming particles that are closer to spherical, and improving the mechanical strength of the purifier; however, too high a rotation speed may also cause excessive wear of the material or unnecessary internal stress. Therefore, the rotation speed cannot be too high. In actual operation, it is necessary to select the appropriate rotation speed according to the specific situation.

[0044] In some specific embodiments of the present invention, the mass concentration of the nitric acid solution is 2%-3%, and the amount of nitric acid solution sprayed is 3%-4% of the total mass of the carrier and active components in the corresponding raw materials. The purpose of spraying nitric acid solution as an adhesive is to increase adhesion and enable the components to bond better.

[0045] In some specific embodiments of the present invention, the water sprayed during the granulation process is preferably deionized water, and the spraying amount is 20%-60% of the total mass of the carrier and the active ingredient in the corresponding raw material, for example, any point value among 20%, 30%, 40%, 50%, 60% or a range value composed of any two point values.

[0046] In some specific embodiments of the present invention, during the granulation process, the mixing temperature of the materials is 20-90°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, etc. The spraying temperature is 20-90°C, for example, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, etc.

[0047] In some specific embodiments of the present invention, the calcination temperature is 300-750°C, for example, any point value among 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, and 750°C, or a range value consisting of any two point values, and the calcination time is 2-4h, for example, any point value among 2h, 2.5h, 3h, 3.5h, and 4h, or a range value consisting of any two point values.

[0048] A third aspect of the present invention provides an application of a purifier as described in any one of the aforementioned embodiments or a purifier prepared by the preparation method of a purifier as described in any one of the aforementioned embodiments in a reforming gas phase and liquid phase dechlorination process or a fuel gas desulfurization process.

[0049] In the following, some embodiments of the present invention are described in detail in conjunction with specific application examples. In the examples, the X-type molecular sieve was purchased from Suzhou Kaifa New Material Technology Co., Ltd., with the brand name NaX raw powder; the sesbania powder was purchased from INNOCHEM, with the brand name SG1; the raw materials used in the examples, if not otherwise specified, can be purchased commercially.

[0050] Example 1

[0051] The raw materials of the inner core are: 50 parts of zinc oxide, 5 parts of magnesium oxide, 30 parts of pseudo-boehmite, 10 parts of kaolin and 5 parts of X-type molecular sieve, and the sesbania powder accounts for 3% of the total weight of the above mixed components.

[0052] The raw materials of the shell are: 50 parts of zinc oxide, 5 parts of magnesium oxide, 30 parts of pseudo-boehmite, 10 parts of kaolin and 5 parts of X-type molecular sieve, and the sesbania powder accounts for 12% of the total weight of the above mixed components.

[0053] The preparation method comprises the following steps:

[0054] (1) stirring and mixing the raw materials of the inner core and the raw materials of the outer shell at room temperature (25° C.) to obtain an inner layer mixture and an outer layer mixture;

[0055] (2) The mixed inner layer mixture is transferred to a disc granulator, and a nitric acid solution and deionized water with a mass fraction of 2% are evenly sprayed. The spraying temperature is room temperature (25° C.), the amount of nitric acid solution sprayed is 3% of the total mass of the active components and carriers in the core raw material, and the amount of deionized water sprayed is 50% of the total mass of the active components and carriers in the core raw material. The disc granulator is operated at a speed of 20 r / min, and the granulation is performed for 0.5 h. The granules are taken out and sieved to obtain spherical particles with a diameter of about 2 mm;

[0056] (3) The uniformly mixed outer layer mixture is transferred to a disc granulator, and the spherical particles of about 2 mm obtained in step (2) are evenly placed in the outer layer mixture, and a nitric acid solution and deionized water with a mass fraction of 3% are evenly sprayed. The spraying temperature is room temperature (25° C.), the amount of nitric acid solution sprayed is 4% of the total mass of the active components and carriers in the shell raw material, and the amount of deionized water sprayed is 60% of the total mass of the active components and carriers in the shell raw material. The disc granulator is first operated at a speed of 30 r / min for 5 min, and then at a speed of 20 r / min for 0.5 h. The particles are taken out and sieved to obtain spherical particles with a diameter of about 3 mm;

[0057] (4) The spherical particles of about 3 mm obtained above are dried and then calcined in a muffle furnace at a temperature of 500° C. for 3 h to obtain the purifier.

[0058] Example 2

[0059] The difference between Example 2 and Example 1 is that in the core material, sesbania powder accounts for 3% of the total weight of the active components and the carrier; in the shell material, sesbania powder accounts for 6% of the total weight of the active components and the carrier; the other conditions are the same as in Example 1.

[0060] Example 3

[0061] The difference between Example 3 and Example 1 is that in the core material, sesbania powder accounts for 3% of the total weight of the active components and the carrier; in the shell material, sesbania powder accounts for 9% of the total weight of the active components and the carrier; the other conditions are the same as in Example 1.

[0062] Example 4

[0063] The difference between Example 4 and Example 1 is that in the core material, sesbania powder accounts for 6% of the total weight of the active components and the carrier; in the shell material, sesbania powder accounts for 12% of the total weight of the active components and the carrier; the other conditions are the same as in Example 1.

[0064] Example 5

[0065] The difference between Example 5 and Example 1 is that in the core material, sesbania powder accounts for 6% of the total weight of the active components and the carrier; in the shell material, sesbania powder accounts for 18% of the total weight of the active components and the carrier; the other conditions are the same as in Example 1.

[0066] Example 6

[0067] The difference between Example 6 and Example 1 is that in the core material, sesbania powder accounts for 3% of the total weight of the active components and the carrier; in the shell material, sesbania powder accounts for 18% of the total weight of the active components and the carrier; the other conditions are the same as in Example 1.

[0068] Example 7

[0069] The difference between Example 7 and Example 1 is that in step (3), after spraying the nitric acid solution and deionized water, the operation of running at a speed of 30 r / min for 5 min was not performed, but granulation was directly performed at 20 r / min for 0.5 h, and the other conditions were the same as those in Example 1.

[0070] Comparative Example 1

[0071] The difference between Comparative Example 1 and Example 1 is that no sesbania powder is added to the raw materials of the core and the shell, and the other conditions are the same as those of Example 1.

[0072] Comparative Example 2

[0073] The difference between Comparative Example 2 and Example 1 is that the amount of sesbania powder added to the raw materials of the core and the shell is 3% of the total mass of the active component and the carrier, and the other conditions are the same as in Example 1.

[0074] Comparative Example 3

[0075] The difference between Comparative Example 3 and Example 1 is that the amount of sesbania powder added to the raw materials of the core and the shell is 6% of the total mass of the active component and the carrier, and the other conditions are the same as Example 1.

[0076] Comparative Example 4

[0077] The difference between Comparative Example 4 and Example 1 is that the amount of sesbania powder added to the raw materials of the core and the shell is 12% of the total mass of the active component and the carrier, and the other conditions are the same as in Example 1.

[0078] Comparative Example 5

[0079] The difference between Comparative Example 5 and Example 1 is that no sesbania powder is added to the core material; the sesbania powder in the shell material accounts for 3% of the total weight of the active component and the carrier; and the other conditions are the same as in Example 1.

[0080] Comparative Example 6

[0081] The difference between Comparative Example 6 and Example 1 is that no sesbania powder is added to the core material; the sesbania powder in the shell material accounts for 6% of the total weight of the active component and the carrier; and the other conditions are the same as in Example 1.

[0082] Comparative Example 7

[0083] The difference between Comparative Example 7 and Example 1 is that no sesbania powder is added to the core material; the sesbania powder in the shell material accounts for 12% of the total weight of the active component and the carrier; and the other conditions are the same as in Example 1.

[0084] Comparative Example 8

[0085] The difference between Comparative Example 8 and Example 1 is that in the core material, sesbania powder accounts for 6% of the total weight of the active component and the carrier; no sesbania powder is added to the shell material; and the other conditions are the same as in Example 1.

[0086] Test example

[0087] The dechlorinating agents prepared in Examples 1-7 and Comparative Examples 1-8 were tested as follows:

[0088] (1) Chlorine capacity test

[0089] The dechlorinating agent was crushed into 20 mesh particles, and then 15 g of the crushed and sieved sample was measured and filled into a quartz reaction tube with a height-to-diameter ratio of 5:1, and placed in a customized heating furnace. The reaction temperature was adjusted to 50°C. In the gas phase penetration test, a mixed gas (including HCl gas and N2) was introduced into the reaction tube, with an inlet concentration of 15000 ppm and an inlet air velocity of 3000 h -1 , a microcomputer coulometric meter was used to sample and measure the HCl concentration of the tail outlet gas, and breakthrough was determined when the outlet gas was ≤0.5ppm. Similarly, the medium in the liquid medium breakthrough test was a solvent liquid of HCl and reforming oil, and the test results are shown in Table 1.

[0090] (2) Determination of average compressive strength

[0091] instrument:

[0092] Particle strength tester: accuracy 1N; range 0~250N; force application speed (5~20)N / s.

[0093] Caliper: accuracy level 0.02mm.

[0094] Electric drying oven: 0℃~300℃.

[0095] Determination steps:

[0096] Dry 50 dechlorination agent samples at (105-120)°C for 1 hour, place in a dryer to cool to room temperature, select 20 samples (the samples are required to be smooth and flat), put them into the particle strength tester one by one, and measure according to the instrument operation steps. Take the arithmetic mean as the measurement result. The test results are shown in Table 1.

[0097] (3) The BET method was used to calculate the percentage of pore volume of 10-50 nm in the inner core of the dechlorinating agent to the total pore volume, and the percentage of pore volume of >50 nm in the outer shell of the dechlorinating agent to the total pore volume. The results are shown in Table 1.

[0098] Table 1

[0099]

[0100] It can be seen from the data in Table 1 that the purifier prepared by the present invention has a gas phase penetration chlorine capacity of up to 51% or more, and a liquid phase penetration chlorine capacity of more than 27%. It has the advantages of high chlorine capacity and wide adaptability to dechlorination raw materials. The purifier prepared by the present invention is superior to the existing purifier with a single pore structure of the inner and outer layers, because the purifier of the present invention has a macropore-medium and small pore structure from the outside to the inside, which is conducive to the penetration of the reaction gas, and can reduce the liquid phase mass transfer resistance and improve the penetration chlorine capacity.

[0101] From the data in Examples 1-6, it can be seen that the ratio of the percentage of the pore-forming agent in the core raw material to the total mass of the carrier and the active component to the percentage of the pore-forming agent in the shell raw material is preferably in the range of 1:2-6, and the effect is better when it is 1:3-4.

[0102] From the comparison of the data of Example 4-5 with that of Example 1, it can be seen that too high a content of pore-forming agent in the raw material of the purifier core is not conducive to the formation of 10-50 nm pores, and the gas phase penetration chlorine capacity is reduced; from the data in Example 2 and Examples 5-6, it can be seen that too low or too high a content of pore-forming agent in the raw material of the purifier shell will lead to a decrease in the proportion of pores larger than 50 nm in the shell, resulting in a decrease in chlorine capacity, so it is necessary to reasonably control the amount of pore-forming agent in the inner and outer layer mixture.

[0103] It can be seen from the data in Example 1 and Example 7 that when coating the purifier shell raw material, first rotating at 20-30 r / min for 1-10 min and then granulating at 10-20 r / min can improve the mechanical strength of the purifier compared to directly granulating at 10-20 r / min.

[0104] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A purifying agent, characterized in that: It comprises an inner core and an outer shell at least partially covering the outer surface of the inner core, wherein the pore volume with a pore size of 10-50 nm in the inner core accounts for ≥64% of the total pore volume; and the pore volume with a pore size of more than 50 nm in the outer shell accounts for ≥24% of the total pore volume.

2. The purifying agent according to claim 1, characterized in that In the shell, the percentage of pore volume with pore diameter greater than 50 nm in the total pore volume is ≥44%.

3. The purifying agent according to claim 1, characterized in that The diameter of the inner core is 1-5 mm, and the thickness of the outer shell accounts for 1 / 4-1 / 2 of the radius of the purifier.

4. The purifying agent according to claim 1, characterized in that The raw materials of the core and the shell both include active components, carriers and pore-forming agents, and meet at least one of the following characteristics (1) to (3): (1) The active component comprises an alkaline earth metal compound and / or a transition metal oxide; (2) The carrier comprises at least one of alumina, molecular sieve and mineral; (3) The pore-forming agent includes methyl cellulose and / or sesbania.

5. The method for preparing the purifying agent according to any one of claims 1 to 4, characterized in that: The following steps are involved: The raw materials of the inner core are mixed and granulated according to a proportion to obtain the inner core, the raw materials of the outer shell are mixed and coated on the outer surface of the inner core, and the purifier is obtained by drying and roasting; In the raw materials of the core, the percentage of the pore-forming agent in the total mass of the active component and the carrier is A; In the raw materials of the shell, the percentage of the pore-forming agent in the total mass of the active component and the carrier is B; and the following conditions are satisfied: 3%≤A≤6%, 6%≤B≤18%, and A:B=1:2-6.

6. The method for preparing the purifying agent according to claim 5, characterized in that: The granulation method of the kernel is rotary granulation, which comprises the following steps: mixing the raw materials of the kernel and placing them in a granulator, spraying nitric acid solution and water in a rotary state for granulation, so as to obtain the kernel; And / or, the raw material of the shell is coated on the outer surface of the core by a rotational granulation method, comprising the following steps: mixing the raw materials of the shell and placing them in a granulator, placing the core into the mixture of the shell, and spraying nitric acid solution and water in a rotating state for granulation.

7. The method for preparing the purifying agent according to claim 6, characterized in that: When the kernel is granulated, the rotation speed of the granulator is 10-20 r / min, and the granulation time is 0.5-5 h.

8. The method for preparing the purifying agent according to claim 6, characterized in that: When coating the raw material of the shell, after the nitric acid solution and water are sprayed in, the granulator is first operated at a speed of 20-30 r / min for 1-10 min, and then granulated at a speed of 10-20 r / min, and the granulation time is 0.5-5 h.

9. The method for preparing the purifying agent according to claim 5, characterized in that: The calcination temperature is 300-750° C., and the calcination time is 2-4 hours.

10. Use of the purifier according to any one of claims 1 to 4 in a reforming gas phase and liquid phase dechlorination process or a fuel gas desulfurization process.

Citation Information

Patent Citations

  • Fluoride-free molten steel purifying agent and preparation method thereof

    CN112981043A

  • Hierarchical pore aluminum oxide material as well as preparation method and application thereof

    CN117756146A