Destressing heat treatment method for thin-wall special-shaped austenitic stainless steel pipe

Through vacuum furnace heat treatment, the problem of difficulty in removing residual stress in thin-walled special-shaped austenitic stainless steel pipes is solved, and the effect of reducing stress and controlling dimensional changes is achieved, and the processing performance is met with high precision and high appearance requirements.

CN118879989APending Publication Date: 2024-11-01TRIO METAL (GZ) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410993596.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-01

Smart Images

  • Figure CN118879989A_ABST
    Figure CN118879989A_ABST
Patent Text Reader

Abstract

A destressing heat treatment method for thin-wall special-shaped austenitic stainless steel pipes comprises the following steps that S1, the thin-wall special-shaped austenitic stainless steel pipes are arranged in a charging tray and dried, and the step S2 is executed; s2, the thin-wall special-shaped austenitic stainless steel pipe and the charging tray are integrally put into a vacuum furnace, and the step S3 is executed; s3, the vacuum furnace is vacuumized; s4, the temperature of the interior of the vacuum furnace is increased to 645 DEG C to 655 DEG C within 200 min to 220 min; s5, heat preservation is conducted for 50 min to 80 min at the temperature of 645 DEG C to 655 DEG C; and S6, naturally cooling, and ending. According to the destressing heat treatment method for the thin-wall special-shaped austenitic stainless steel pipe, the thin-wall special-shaped austenitic stainless steel pipe is dried firstly, then vacuumized, then heated to 645-655 DEG C within the range of 200-220 min and then subjected to heat preservation for 50-80 min, and the residual stress of the obtained thin-wall special-shaped austenitic stainless steel pipe subjected to heat treatment ranges from 29 Mpa to 105 Mpa; and the size change after processing is from 4.075 mm to 4.230 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of special-shaped stainless steel pipes, and in particular to a stress relief heat treatment method for thin-wall special-shaped austenitic stainless steel pipes. Background Art

[0002] Austenitic stainless steel has an austenitic structure at room temperature. It is non-magnetic and has high toughness and plasticity. Its strength is relatively low and it is impossible to strengthen it through phase transformation. However, it can be hardened through cold working, and the increase in strength and the decrease in plasticity are very obvious. Since austenitic stainless steel can only improve its strength through deformation strengthening, the higher the strength, the greater the deformation and the greater the residual stress. Since austenitic stainless steel will produce stress release during subsequent processing, such as laser cutting, CNC processing, etc., the subsequent processing of pipe size changes will increase and be non-uniform.

[0003] At present, stainless steel plates and stainless steel ingots mostly use mechanical stress relief methods, such as vibration method and pressure method. The vibration method uses a vibrator or vibration platform to apply periodic vibration loads to the structural parts, causing them to deform slightly within the elastic range and release internal stress; the pressure method uses hydraulic presses, pressure vessels and other equipment to apply a certain static or dynamic pressure to the structural parts, causing them to deform plastically or elastically and eliminate internal stress. Moreover, both the vibration method and the pressure method are prone to cause changes in product size and damage to product appearance, so they are not used for products with high precision and appearance requirements. The stress relief method for ordinary austenitic stainless steel round tubes is mostly heat treatment under non-vacuum conditions and rapid cooling in air, which is prone to cause surface oxidation and is not suitable for products with high appearance requirements.

[0004] Special-shaped austenitic stainless steel pipes are mainly drawn by fixed dies or roller dies. Due to their non-complete symmetry, the deformation resistance of the pipe is also unevenly distributed in the radial direction, resulting in uneven distribution of residual stress in the pipe. For thick-walled special-shaped austenitic stainless steel pipes with a wall thickness generally greater than 6mm and a wall thickness to outer diameter ratio less than 10%, the residual stress is generally mainly in the diameter direction, which usually causes changes in radial dimensions during processing, such as diameter shrinkage or expansion, changes in processing groove width, etc. Thin-walled stainless steel pipes refer to stainless steel pipes with a wall thickness to outer diameter ratio of no more than 10%, and the wall thickness is generally not more than 6mm. Thin-walled pipe products have high requirements for size and appearance, and the grooving on the pipe requires an accuracy of 0.01mm. Compared with thick-walled special-shaped austenitic stainless steel pipes, thin-walled special-shaped austenitic stainless steel pipes generally need to undergo multiple cold drawing processes to reduce the wall thickness, so the residual stress along the longitudinal direction of the pipe wall (i.e., the length direction) is greater, and the length direction size changes are relatively large during precision processing. When cutting a fixed length of pipe, the length of the pipe will change, and when slotting the pipe, the length of the slot will also change. At present, it is relatively difficult to relieve stress of thick-walled special-shaped austenitic stainless steel pipes, so it is even more difficult to relieve stress of thin-walled special-shaped austenitic stainless steel pipes.

[0005] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe to solve the shortcomings of the prior art. Summary of the invention

[0006] The purpose of the present invention is to avoid the shortcomings of the prior art and provide a stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipes. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipes effectively reduces residual stress, thereby reducing the size change of subsequent processing.

[0007] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0008] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is provided, which is carried out by the following steps:

[0009] S1, placing thin-walled special-shaped austenitic stainless steel tubes in a tray and drying them, and then entering S2;

[0010] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0011] S3, evacuate the vacuum furnace;

[0012] S4. Raise the temperature inside the vacuum furnace to 645°C to 655°C within 200min to 220min;

[0013] S5. Keep warm at 645℃~655℃ for 50min~80min;

[0014] S6, natural cooling, end.

[0015] In S4, the temperature inside the vacuum furnace is raised to 650° C. within 210 minutes.

[0016] Preferably, the above S5 is specifically to keep the temperature at 650° C. for 60 minutes.

[0017] Preferably, the above S6 specifically comprises taking out the thin-walled special-shaped austenitic stainless steel tube after naturally cooling to 50°C.

[0018] Preferably, the above S3 is to evacuate the vacuum furnace for 20 min to 60 min, and the vacuum degree is less than or equal to 3×10 - 3 pa.

[0019] Preferably, the above S1 specifically comprises placing the thin-walled special-shaped austenitic stainless steel tubes in a tray and heating them to 50° C. to 80° C., drying them for 3 min to 20 min, and then entering S2.

[0020] Preferably, the above S3 is to evacuate the vacuum furnace for 40 minutes, and the vacuum degree is less than or equal to 2×10 -3 pa.

[0021] Preferably, the above S1 specifically comprises placing the thin-walled special-shaped austenitic stainless steel tubes in a material tray and heating them to 65° C., drying them for 5 minutes, and then entering S2.

[0022] The tray is divided into an inner tray and an outer tray, and in S2, the inner tray is close to the inner wall of the vacuum furnace, the outer tray is parallel to the inner tray, and the outer tray is far away from the inner wall of the vacuum furnace.

[0023] Preferably, the length and width of the above-mentioned tray are both A, and 50cm≤A≤70cm;

[0024] A first heat dissipation zone is arranged in the inner material tray, and no thin-walled special-shaped austenitic stainless steel tube is placed in the first heat dissipation zone. The first heat dissipation zone is close to the inner wall of the vacuum furnace, and the length of the first heat dissipation zone is A, and the width of the first heat dissipation zone is 0.25A.

[0025] A second heat dissipation zone is arranged in the outer material tray, in which no thin-walled special-shaped austenitic stainless steel tube is placed, and the second heat dissipation zone is close to the inner material tray, and the length of the second heat dissipation zone is 0.5A, and the width of the second heat dissipation zone is 0.25A.

[0026] Preferably, the outer material tray and the inner material tray are placed in layers in the working area of ​​the vacuum furnace; and the inner material tray and the outer material tray are placed parallel to the central axis of the working area.

[0027] Preferably, the inner material tray and the outer material tray are placed parallel to the central axis of the working area.

[0028] Preferably, the distance between the inner material tray and the adjacent inner material tray is 8 cm to 12 cm.

[0029] Preferably, the distance between the outer material tray and the adjacent outer material tray is 8 cm to 12 cm.

[0030] Preferably, the diameter of the cylindrical region is 90 cm, and the length of the cylindrical region is 120 cm.

[0031] The residual stress of the thin-walled special-shaped austenitic stainless steel pipe after heat treatment is 29Mpa-105Mpa, and the size change after processing is 4.075mm-4.230mm.

[0032] The shape of the thin-walled special-shaped austenitic stainless steel tube of the present invention is a closed thin-walled special-shaped austenitic stainless steel tube obtained by virtually cutting a virtual circular tube by a virtual plane, and the cross-sectional edge of the thin-walled special-shaped austenitic stainless steel tube after virtual cutting is closed by a circular arc and a line segment, and the circular arc is a major arc;

[0033] Preferably, the wall thickness of the above-mentioned thin-walled special-shaped austenitic stainless steel tube is 0.20 mm to 0.4 mm.

[0034] Preferably, the length of the thin-walled special-shaped austenitic stainless steel tube is 140 mm to 150 mm.

[0035] Preferably, the outer diameter of the virtual circular tube is 6.50 mm to 8.00 mm.

[0036] The invention discloses a stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe, which comprises the following steps: S1, placing the thin-walled special-shaped austenitic stainless steel pipe in a material tray and drying it, and entering S2; S2, placing the thin-walled special-shaped austenitic stainless steel pipe and the material tray as a whole into a vacuum furnace, and entering S3; S3, evacuating the vacuum furnace; S4, heating the inside of the vacuum furnace to 645°C to 655°C within 200min to 220min; S5, keeping the temperature at 645°C to 655°C for 50min to 80min; S6, cooling naturally, and ending. The stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe of the present invention first dries the thin-walled special-shaped austenitic stainless steel pipe, then evacuates the pipe, and then heats it to 645°C to 655°C within a range of 200min to 220min, and then keeps the temperature for 50min to 80min, so that the residual stress of the thin-walled special-shaped austenitic stainless steel pipe after the heat treatment is 29Mpa to 105Mpa; and the size change after processing is 4.075mm to 4.230mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 Schematic diagram of the inner and outer trays placed in the cylindrical area.

[0038] Figure 2 This is a picture of the inner and outer trays placed in the cylindrical area during actual production.

[0039] Figure 3 This is a picture of the material tray being placed in actual production.

[0040] Figure 4 This is the front view of a thin-walled special-shaped austenitic stainless steel tube.

[0041] Figure 5 It is the right view of thin-walled special-shaped austenitic stainless steel tube.

[0042] Figure 6 This is the residual stress measurement site map of thin-walled special-shaped austenitic stainless steel pipe.

[0043] Figure 7 This is the residual stress measurement site map of thin-walled special-shaped austenitic stainless steel pipe.

[0044] Figure 8 This is a diagram of the window measurement sites for thin-walled special-shaped austenitic stainless steel tubes. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is further described in conjunction with the following embodiments.

[0046] Example 1

[0047] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0048] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 50°C, dry it for 20 minutes, and enter S2;

[0049] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0050] S3, evacuate the vacuum furnace for 20 minutes, and the vacuum degree is 2.99×10 -3 pa;

[0051] S4. Raise the temperature inside the vacuum furnace to 645°C at a uniform rate within 200 minutes;

[0052] S5, keep warm at 645℃ for 80min;

[0053] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0054] The tray is divided into an inner tray and an outer tray, and in S2, the inner tray is close to the inner wall of the vacuum furnace, the outer tray is parallel to the inner tray, and the outer tray is far away from the inner wall of the vacuum furnace; the length and width of the tray are both A, and A is 60 cm.

[0055] A first heat dissipation zone is provided in the inner material tray, in which no thin-walled special-shaped austenitic stainless steel tube is placed, and the first heat dissipation zone is close to the inner wall of the vacuum furnace, and the length of the first heat dissipation zone is 60 cm, and the width of the first heat dissipation zone is 15 cm; a second heat dissipation zone is provided in the outer material tray, in which no thin-walled special-shaped austenitic stainless steel tube is placed, and the second heat dissipation zone is close to the inner material tray, and the length of the second heat dissipation zone is 30 cm, and the width of the second heat dissipation zone is 15 cm. The material trays are placed in layers in the working area of ​​the vacuum furnace. The vacuum furnace used in the present invention is a structure with a cylindrical space, and the central axis of the cylindrical space is parallel to the ground. The working area is located inside the cylindrical space, and the working area is provided with a multi-layer placement rack, and the material trays are placed on the placement rack in parallel and layers. The diameter of the working area is 90 cm, and the length of the working area is 120 cm.

[0056] It should be noted that the function of the first heat dissipation zone and the second heat dissipation zone is to increase the heat dissipation between the inner material tray and the outer material tray to strengthen the heat dissipation between the materials. If there is no heat dissipation zone, it is easy to cause uneven temperature on each layer of the material rack. Figure 1-Figure 2 shown.

[0057] The spacing between the inner material tray and the adjacent inner material tray is 10cm, and the spacing between the outer material tray and the adjacent outer material tray is 10cm. Based on the cylindrical area size of the present invention, a total of 8 layers of inner material trays and outer material trays are placed respectively. However, if the material trays are placed at the bottom of the cylindrical area, the material trays absorb more heat, which can easily lead to uneven temperatures of the bottom material trays. Therefore, in this embodiment, no material trays are placed at the bottom, and only 7 layers of inner material trays and outer material trays are placed respectively, and two layers of thin-walled special-shaped austenitic stainless steel tubes are placed in each layer of inner material trays and outer material trays. The inner material tray and the outer material tray are placed parallel to the central axis of the cylindrical area, such as Figure 3 shown.

[0058] The shape of the thin-walled special-shaped austenitic stainless steel tube of the present invention is a closed thin-walled special-shaped austenitic stainless steel tube obtained by virtually cutting a virtual circular tube by a virtual plane, and the cross-sectional edge of the thin-walled special-shaped austenitic stainless steel tube after virtual cutting is closed by a circular arc and a line segment, and the circular arc is a major arc; the wall thickness of the thin-walled special-shaped austenitic stainless steel tube is 0.20mm-0.4mm; the length of the thin-walled special-shaped austenitic stainless steel tube is 140mm-150mm; the outer diameter of the virtual circular tube is 6.50mm-8.00mm, such as Figure 4-Figure 5 As shown, the thin-walled special-shaped austenitic stainless steel tube of the present invention is mainly used for electronic pen housing and fountain pen housing.

[0059] Compared with the circular austenitic stainless steel tube, the residual stress of the thin-walled special-shaped austenitic stainless steel tube of the present invention is significantly higher than that of the circular austenitic stainless steel tube. The vibration aging and other heat treatments in the prior art are difficult to reduce the residual stress to a low level. The stress relief heat treatment method of the present invention can reduce the residual stress of the thin-walled special-shaped austenitic stainless steel tube of this shape and size to 29Mpa~105Mpa; the size change after processing is 4.075mm~4.230mm.

[0060] Example 2

[0061] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0062] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 80°C, dry it for 10 minutes, and enter S2;

[0063] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0064] S3, evacuate the vacuum furnace for 60 minutes, and the vacuum degree is 2.5×10 -3 pa;

[0065] S4. Raise the temperature of the vacuum furnace to 655°C at a uniform rate within 220 minutes;

[0066] S5, keep warm at 655℃ for 50min;

[0067] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0068] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0069] Example 3

[0070] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0071] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0072] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0073] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0074] S4, uniformly raise the temperature inside the vacuum furnace to 650°C within 210 minutes;

[0075] S5, keep warm at 650℃ for 60min;

[0076] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0077] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0078] Comparative Example 1

[0079] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0080] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0081] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0082] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0083] S4. Raise the temperature inside the vacuum furnace to 300°C within 70 minutes and keep it at this temperature for 60 minutes;

[0084] S5. Raise the temperature inside the vacuum furnace from 300°C to 680°C within 70 minutes and keep it warm for 70 minutes;

[0085] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0086] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0087] Comparative Example 2

[0088] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0089] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0090] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0091] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0092] S4. Raise the temperature inside the vacuum furnace to 450°C within 70 minutes and keep it at this temperature for 70 minutes;

[0093] S5. Raise the temperature inside the vacuum furnace from 450°C to 680°C within 60 minutes and keep it warm for 70 minutes;

[0094] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0095] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the tray and the placement of the tray in the vacuum furnace in this embodiment are the same as those in Example 1. At the same time, each tray in the vacuum furnace uses a cover pressing sheet to press the thin-walled special-shaped austenitic stainless steel tubes.

[0096] Comparative Example 3

[0097] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0098] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0099] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0100] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0101] S4. Raise the temperature inside the vacuum furnace to 650°C within 180 minutes;

[0102] S5, keep warm at 650℃ for 60min;

[0103] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0104] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0105] Comparative Example 4

[0106] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0107] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0108] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0109] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0110] S4, uniformly raise the temperature inside the vacuum furnace to 650°C within 210 minutes;

[0111] S5, keep warm at 650℃ for 40min;

[0112] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0113] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0114] Comparative Example 5

[0115] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0116] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0117] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0118] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0119] S4, uniformly raise the temperature inside the vacuum furnace to 650°C within 230 minutes;

[0120] S5, keep warm at 650℃ for 60min;

[0121] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0122] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0123] Comparative Example 6

[0124] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0125] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0126] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0127] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0128] S4. Raise the temperature of the vacuum furnace to 660°C at a uniform rate within 210 minutes;

[0129] S5, keep warm at 660°C for 60 min;

[0130] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0131] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0132] Comparative Example 7

[0133] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0134] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0135] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0136] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0137] S4. Raise the temperature of the vacuum furnace to 640°C at a uniform rate within 210 minutes;

[0138] S5, keep warm at 640℃ for 60min;

[0139] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0140] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0141] Comparative Example 8

[0142] A stress relief heat treatment method for a thin-walled special-shaped austenitic stainless steel pipe is carried out by the following steps:

[0143] S1, place the thin-walled special-shaped austenitic stainless steel tube in a tray and heat it to 65°C, dry it for 5 minutes, and enter S2;

[0144] S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3;

[0145] S3, evacuate the vacuum furnace for 40 minutes, and the vacuum degree is 2.0×10 -3 pa;

[0146] S4. Raise the temperature of the vacuum furnace to 650°C at a uniform rate within 210 minutes;

[0147] S5, keep warm at 650℃ for 60min;

[0148] S6. After the temperature naturally drops to 50°C, take out the thin-walled special-shaped austenitic stainless steel tube and finish.

[0149] The thin-walled special-shaped austenitic stainless steel tube of this embodiment has no heat dissipation zone in the inner tray and the outer tray, and the placement of the tray in the vacuum furnace is the same as that in Example 1.

[0150] The placement of the thin-walled special-shaped austenitic stainless steel tubes on the material tray and the placement of the material tray in the vacuum furnace in this embodiment are the same as those in Example 1.

[0151] Effect example

[0152] 1. Residual stress measurement

[0153] The stress relief heat treatment method of Examples 1 to 3 and Comparative Examples 1 to 8 was used to Figure 4-Figure 5 The specifications of the special-shaped thin-walled tube are stress relieved, and then after the stress relief heat treatment method, Figure 6 and Figure 8 Select C1-A1, C1-A2, C2-A1, C2-A2 as the residual stress measurement points, and Figure 4-Figure 8 The unit is mm. An X-ray residual stress meter is used to measure the residual stresses at the four measuring points C1-A1, C1-A2, C2-A1 and C2-A2, and 5 samples are taken for each stress relief heat treatment method, as shown in Tables 1 and 2.

[0154] Table 1. Residual stress values ​​of the blank group and samples of Examples 1 to 3, in MPa.

[0155]

[0156]

[0157] Table 2. Residual stress values ​​of samples from Comparative Examples 1 to 8, in MPa.

[0158]

[0159] The blank group is a thin-walled austenitic stainless steel tube that has not been subjected to stress relief heat treatment. The standard value of residual stress for thin-walled tubes is ±170Mpa, and the ideal value is ±100Mpa. When the stress is positive, it is tensile stress, and when the stress is negative, it is compressive stress.

[0160] From the data in Table 1 and Table 2, it can be seen that the maximum residual stress of Examples 1-3 of the present invention is only 102Mpa, 104Mpa and 105Mpa, and the average residual stress is 69Mpa, 64Mpa and 68Mpa, respectively, which are basically excellent ideal values. Compared with Comparative Examples 1-8, the residual stress of the present invention can be significantly reduced.

[0161] 2. Window width measurement

[0162] The thin-walled special-shaped austenitic stainless steel tube after the stress relief heat treatment method of Examples 1 to 3 and Comparative Examples 1 to 8 is subjected to precision laser cutting and windowing, such as Figure 6 and Figure 6 The unit is mm, and then the P1, P2, P3, P4, P5 and P6 measuring points are measured using a two-dimensional image measuring instrument, and 8 samples are taken for each stress relief heat treatment method.

[0163] Table 1. Measurement values ​​of blank group and samples of Examples 1 to 3, in mm.

[0164]

[0165]

[0166] Table 2. Measurement values ​​of samples of Comparative Examples 1 to 8, in mm.

[0167]

[0168]

[0169] The blank group is the window opening data of thin-walled special-shaped austenitic stainless steel tubes without stress relief heat treatment. It should be noted that the standard value of the window opening of thin-walled special-shaped thin-walled tubes is 4.07mm-4.23mm.

[0170] It can be seen from the data in Table 3 and Table 4 that some of the window sizes of Comparative Examples 1 to Comparative Examples 8 are outside the range of 4.07 mm to 4.23 mm, while all the window sizes of Examples 1 to 3 of the present invention are within the range of 4.07 mm to 4.23 mm.

[0171] In summary, after using the stress relief heat treatment method of the present invention, the residual stress of the thin-walled and thin-walled special-shaped austenitic stainless steel pipe is significantly reduced, all of which are within the target range of ±170Mpa, and basically within the extremely optimal ideal value of ±100Mpa. Therefore, the deformation caused by stress release during the laser precision cutting process makes the window size opened enter the target range of 4.07mm-4.23mm, and the processing performance is improved. Although the residual stress of the comparative example is reduced compared with the blank group, it has not completely entered the range of ±170Mpa. There is still a large stress release during the cutting process, resulting in deformation after cutting, poor cutting performance, and the size exceeds the predetermined target range of 4.07mm-4.23mm. It can be seen that only with the stress relief heat treatment method within the scope of the present invention can the best stress relief effect be achieved and the performance after cutting be guaranteed.

[0172] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe, characterized in that: The following steps are performed: S1, placing thin-walled special-shaped austenitic stainless steel tubes in a tray and drying them, and then entering S2; S2, placing the thin-walled special-shaped austenitic stainless steel tube and the material tray into a vacuum furnace as a whole, and entering S3; S3, evacuate the vacuum furnace; S4. Raise the temperature inside the vacuum furnace to 645°C to 655°C within 200min to 220min; S5. Keep warm at 645℃~655℃ for 50min~80min; S6, natural cooling, end.

2. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 1, characterized in that: In S4, the temperature inside the vacuum furnace is raised to 650° C. within 210 minutes.

3. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 1, characterized in that: The S5 is specifically to keep the temperature at 650° C. for 60 minutes.

4. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 1, characterized in that: The S6 specifically comprises taking out the thin-walled special-shaped austenitic stainless steel tube after the temperature is naturally reduced to 50°C.

5. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 1, characterized in that: The S3 is to evacuate the vacuum furnace for 20 minutes to 60 minutes, and the vacuum degree is less than or equal to 3×10 -3 pa; Specifically, S1 is to place the thin-walled special-shaped austenitic stainless steel tubes in a tray and heat them to 50° C. to 80° C., dry them for 3 min to 20 min, and then enter S2.

6. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 5, characterized in that: The S3 is to evacuate the vacuum furnace for 40 minutes, and the vacuum degree is less than or equal to 2×10 -3 pa; Specifically, S1 is to place the thin-walled special-shaped austenitic stainless steel tubes in a tray and heat them to 65° C., dry them for 5 minutes, and then enter S2.

7. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 1, characterized in that: The material tray is divided into an inner material tray and an outer material tray, and in S2, the inner material tray is close to the inner wall of the vacuum furnace, the outer material tray is parallel to the inner material tray, and the outer material tray is far away from the inner wall of the vacuum furnace; The length and width of the tray are both A, and 50cm≤A≤70cm; A first heat dissipation zone is provided in the inner material tray, the first heat dissipation zone does not contain a thin-walled special-shaped austenitic stainless steel tube, and the first heat dissipation zone is close to the inner wall of the vacuum furnace, and the length of the first heat dissipation zone is A, and the width of the first heat dissipation zone is 0.25A; A second heat dissipation zone is arranged in the outer material tray, in which no thin-walled special-shaped austenitic stainless steel tube is placed, and the second heat dissipation zone is close to the inner material tray, and the length of the second heat dissipation zone is 0.5A, and the width of the second heat dissipation zone is 0.25A.

8. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 7, characterized in that: The outer material tray and the inner material tray are both placed in layers in the working area of ​​the vacuum furnace; and the inner material tray and the outer material tray are placed parallel to the central axis of the working area.

9. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 8, characterized in that: The distance between the inner material tray and the adjacent inner material tray is 8cm to 12cm; The distance between the outer material tray and the adjacent outer material tray is 8cm to 12cm.

10. The stress relief heat treatment method for thin-walled special-shaped austenitic stainless steel pipe according to claim 1, characterized in that: The residual stress of the thin-walled special-shaped austenitic stainless steel pipe after heat treatment is 29Mpa~105Mpa; and the size change after processing is 4.075mm~4.230mm; The shape of the thin-walled special-shaped austenitic stainless steel tube is a closed thin-walled special-shaped austenitic stainless steel tube obtained by virtually cutting a virtual circular tube by a virtual plane, and the cross-sectional edge of the thin-walled special-shaped austenitic stainless steel tube after virtual cutting is closed by a circular arc and a line segment, and the circular arc is a major arc; The wall thickness of the thin-walled special-shaped austenitic stainless steel tube is 0.20 mm to 0.40 mm; The length of the thin-walled special-shaped austenitic stainless steel tube is 140 mm to 150 mm; The outer diameter of the virtual circular tube is 6.50 mm to 8.00 mm.