Recovery method of carbonate type sandstone uranium ore
Through the adjustment of the multi-stage leaching process, combined with CO2, O2, bicarbonate, oxygen and sulfuric acid and other agents, the problems of low leaching rate of carbonate-type sandstone uranium ore and long mining area cycle are solved, and high-efficiency uranium resource recovery is achieved .
Patent Information
- Application Number
- CN202410929807.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The carbonate-type sandstone uranium ore has a low leaching rate in the neutral leaching process, and the leaching period in the mining area is long, making it difficult to effectively recover uranium resources.
A multi-stage leaching process is adopted, including the first leaching, the second leaching and the transformation leaching. By adjusting the leaching agent composition and leaching conditions, the carbonate content and pH adjustment are gradually reduced, so as to achieve efficient dissolution and migration of uranium minerals. Specific steps include: using CO2 and O2 in the first leaching stage, adding bicarbonate in the second leaching stage, using oxygen and inorganic acid in the first stage, and using sulfuric acid and hydrogen peroxide in the third leaching stage.
The leaching rate of carbonate-type sandstone uranium ore has been improved by more than 15%, shortened the leaching cycle in the mining area, and achieved efficient uranium recovery, making it suitable for sandstone uranium ore with high carbonate content in the reservoir.
Smart Images

Figure CN118880077A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of uranium resource utilization, and in particular relates to a method for recovering carbonate-type sandstone uranium ore. Background Art
[0002] In-situ leaching uranium mining technology is mainly divided into neutral leaching technology and acid leaching technology according to the type of leaching agent. Among them, the neutral leaching process is suitable for sandstone uranium deposits with high carbonate content (CO2> 2%), or HCO3 in ore layer water. - For sandstone uranium deposits with a concentration > 800 mg / L, the acid leaching process is suitable for deposits with low carbonate content.
[0003] For the sandstone uranium ore with high carbonate content, the neutral leaching process includes two stages: the first stage uses CO2 and O2 as leaching agents, O2 oxidizes the tetravalent uranium in the ore layer, and CO2 fully reacts with the carbonate in the ore layer to generate sufficient HCO3 - , to achieve the conditions for uranium mineral oxidation and dissolution migration; in the second stage, as the carbonate minerals in the ore layer are exhausted, the leaching agent formula is adjusted to CO2, O2 and NaHCO3, or CO2, O2 and NH4HCO3, the pH value is controlled at 6.5-7.0, and the HCO3 - The concentration is >800mg / L until the mining area is finally mined.
[0004] When the above-mentioned neutral leaching process mining area is finally mined, most of them have co-precipitation of calcite and uranium minerals. The carbonate content in the ore is significantly higher than that in the surrounding rock. Under the conditions of CO2 and O2 leaching processes, the calcite minerals are dissolved and the uranium element is reactivated and migrated, but the leaching rate is low, with an average leaching rate of 50% to 75% (including the recovery of extra-surface ore). Summary of the invention
[0005] The purpose of the present invention is to provide a method for recovering carbonate-type sandstone uranium ore. The recovery method for carbonate-type sandstone uranium ore provided by the present invention directly increases the leaching rate by more than 15% compared with conventional methods.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for recovering carbonate sandstone uranium ore, comprising the following steps:
[0008] (1) Using a first leaching agent to perform a first leaching on a carbonate sandstone uranium ore to obtain a leaching solution until HCO3 in the leaching solution is - The concentration of is reduced to 800 mg / L; the first leaching agent includes CO2, O2 and water;
[0009] (2) using a second leaching agent to perform a second leaching on the carbonate sandstone uranium ore after the first leaching to obtain a leachate, wherein HCO3 - The concentration is not less than 800 mg / L; the second leaching agent includes CO2, O2, water and bicarbonate; the bicarbonate includes one or more of NaHCO3, NH4HCO3, KHCO3 and Mg(HCO3)2;
[0010] (3) after the carbonate sandstone uranium ore after the second leaching is subjected to transformation preparation using a transformation preparation leaching agent, the carbonate sandstone uranium ore after the transformation preparation is subjected to transformation leaching using a transformation preparation leaching agent to obtain a leachate until the pH value of the leachate is reduced to 2; the transformation preparation leaching agent comprises a transformation preparation oxidant and water; the transformation preparation oxidant comprises one or two of oxygen and hydrogen peroxide; the transformation leaching agent comprises an inorganic acid and water;
[0011] (4) performing a third leaching on the carbonate sandstone uranium ore after the transition leaching using a third leaching agent; the third leaching agent comprises H2SO4, H2O2 and water.
[0012] Preferably, the first leaching includes an initial leaching period and a peak leaching period performed sequentially; in the initial leaching period, the concentration of CO2 in the first leaching agent is 400-600 mg / L, and the concentration of O2 is 100-200 mg / L.
[0013] Preferably, during the peak period of leaching, the concentration of CO2 in the first leaching agent is 600-800 mg / L, and the concentration of O2 is 150-300 mg / L.
[0014] Preferably, the leaching preparation is also included before the initial stage of leaching; the leaching preparation is: using a leaching preparation agent to dredge the ore layer; the leaching preparation agent includes CO2 and water.
[0015] Preferably, the concentration of CO2 in the leaching preparation agent is 200-400 mg / L.
[0016] Preferably, the second leaching comprises a mid-leaching period and a mid-late leaching period, which are performed sequentially; in the mid-leaching period, the concentration of CO2 in the second leaching agent is 400-600 mg / L, the concentration of O2 is 100-200 mg / L, and the concentration of bicarbonate is 100-200 mg / L. - The concentration is above 1000mg / L.
[0017] Preferably, in the middle and late stages of leaching, the concentration of CO2 in the second leaching agent is 300-400 mg / L, the concentration of O2 is 100-200 mg / L, and the concentration of bicarbonate is based on the concentration of HCO3 in the leaching agent. -The concentration is 800-1200 mg / L.
[0018] Preferably, the concentration of the transformation preliminary oxidant in the transformation preliminary leaching agent is 100 to 200 mg / L.
[0019] Preferably, the concentration of the inorganic acid in the transition leaching agent is 2 to 3 g / L.
[0020] Preferably, the concentration of H2SO4 in the third leaching agent is 6-10 g / L, and the concentration of H2O2 is 0.2-0.5 g / L.
[0021] The present invention provides a method for recovering carbonate sandstone uranium ore. The recovery method provided by the present invention includes a first leaching stage, a second leaching stage, and a third leaching stage after the leaching process is transformed; the node control of different leaching stages is based on the HCO3 - Concentration changes and concentration values: The first leaching stage ends with HCO3 in the leaching solution - After the concentration reaches the peak, it gradually decreases to 800 mg / L as the control node; the second leaching stage ends and HCO3 is added - Still can't maintain HCO3 in the leaching solution - The control node is when the concentration is 800 mg / L; the end of the leaching process transformation stage is when the pH value drops to 2; the end of the third leaching stage is when the uranium concentration in the leaching solution is lower than the economically recoverable concentration (such as Figure 1 shown).
[0022] The beneficial effects of the phased efficient recovery method provided by the present invention mainly include two aspects: on the one hand, the leaching rate of the carbonate sandstone uranium ore mining area is increased by more than 15% (the leaching rate is directly increased by more than 15%, rather than increasing the original leaching rate by more than 15%, for example, the leaching rate is increased from 70% to more than 85%, rather than more than 115% of 70%): the present invention first adopts neutral leaching to solve the problem of high carbonate content in the early and middle stages of leaching of carbonate sandstone uranium ore, and produces uranium leaching complexing agent HCO3 by adding CO2 to dissolve carbonate minerals and adjusting the leaching pH value. - , killing two birds with one stone; with the gradual consumption of carbonate minerals, the carbonate content of the ore deposit is low enough to meet the requirements of the acid leaching process, and then the leaching process transformation method is adopted to smoothly transition the uranium leaching interval from the neutral leaching interval to the acid leaching interval; after that, the acid leaching process is adopted to dissolve the acid-soluble chemical blockages formed in the ore layer during the neutral leaching stage, dredge the ore layer, dissolve the surface inclusions of uranium minerals, realize the efficient leaching of the remaining uranium, and effectively improve the uranium leaching rate.
[0023] On the other hand, the present invention shortens the leaching period of carbonate sandstone uranium mining area by 3 to 5 years: the leaching period of the existing in-situ leaching uranium mining process is generally 8 to 12 years. After the leaching process transformation stage, acid leaching is adopted to accelerate the dissolution of uranium minerals, increase the leaching reaction rate, reduce the tailing in the late stage of neutral leaching, and shorten the service life of the mining area.
[0024] The invention timely adjusts the leaching method according to different leaching stages of carbonate sandstone uranium ore, adapts to the change of ore layer lithology, effectively controls the chemical blockage in each leaching stage, solves the problem of low recovery rate of carbonate sandstone uranium ore under neutral leaching conditions, "eats up and squeezes out" the remaining uranium, improves the leaching rate, shortens the uranium mine development cycle, realizes efficient uranium recovery, and is particularly suitable for mining sandstone uranium ore with high reservoir carbonate content and original ore layer water bicarbonate concentration lower than 500 mg / L. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 The process flow chart of the recovery method of carbonate sandstone uranium ore of the present invention is as follows;
[0027] Figure 2 It is the leaching transformation principle diagram of the recovery method of the present invention;
[0028] Figure 3 The concentration changes of uranium, bicarbonate and sulfate ions in the leaching solution at different stages of Example 1 of the present invention are shown;
[0029] Figure 4 The uranium concentration and cumulative leaching rate in the leaching solution at different stages of Example 1 of the present invention are shown. DETAILED DESCRIPTION
[0030] The present invention provides a method for recovering carbonate sandstone uranium ore, comprising the following steps:
[0031] (1) Using a first leaching agent to perform a first leaching on a carbonate sandstone uranium ore to obtain a leaching solution until HCO3 in the leaching solution is - The concentration of is reduced to 800 mg / L; the first leaching agent includes CO2, O2 and water;
[0032] (2) using a second leaching agent to perform a second leaching on the carbonate sandstone uranium ore after the first leaching to obtain a leachate, wherein HCO3 -The concentration is not less than 800 mg / L; the second leaching agent includes CO2, O2, water and bicarbonate; the bicarbonate includes one or more of NaHCO3, NH4HCO3, KHCO3 and Mg(HCO3)2;
[0033] (3) after the carbonate sandstone uranium ore after the second leaching is subjected to transformation preparation using a transformation preparation leaching agent, the carbonate sandstone uranium ore after the transformation preparation is subjected to transformation leaching using a transformation preparation leaching agent to obtain a leachate until the pH value of the leachate is reduced to 2; the transformation preparation leaching agent comprises a transformation preparation oxidant and water; the transformation preparation oxidant comprises one or two of oxygen and hydrogen peroxide; the transformation leaching agent comprises an inorganic acid and water;
[0034] (4) performing a third leaching on the carbonate sandstone uranium ore after the transition leaching using a third leaching agent; the third leaching agent comprises H2SO4, H2O2 and water.
[0035] The present invention uses a first leaching agent to perform a first leaching on carbonate sandstone uranium ore to obtain a leaching solution until HCO3 in the leaching solution is - The concentration of HCO3 in the leachate is reduced to 800 mg / L. In the present invention, the first leaching preferably includes an initial leaching period and a peak leaching period performed sequentially; the first leaching is preferably a flowing leaching. In the present invention, the concentration of HCO3 in the leachate increases first and then decreases. When the concentration of HCO3 in the leachate increases to 800 mg / L, it enters the peak leaching period from the initial leaching period; when the concentration of HCO3 in the leachate increases to 800 mg / L, it enters the peak leaching period from the initial leaching period; - When the concentration drops from a high value to 800 mg / L, the peak leaching period ends (the first leaching also ends).
[0036] In the present invention, in the initial stage of leaching, the concentration of CO2 in the first leachant is preferably 400-600 mg / L, more preferably 450-550 mg / L, and further preferably 500 mg / L, and the concentration of O2 is preferably 100-200 mg / L, more preferably 120-180 mg / L, and further preferably 140-160 mg / L.
[0037] In the present invention, in the initial stage of leaching, the mass ratio of the first leaching agent to the carbonate sandstone uranium ore is preferably 5-10:1000-2000, more preferably 5-8:1000-2000, and further preferably 5:1000.
[0038] The present invention simultaneously monitors the pH value and HCO3 of the leaching solution at the initial stage of leaching. - concentration and uranium concentration and its changes (Ca 2+ Mg 2+ , K + 、SO42- and Si ions or elements), during this period, the pH value of the leaching solution dropped to 6.5-7.5, HCO3 - The concentration rises to above 500 mg / L, and the uranium concentration gradually increases. When the ore grade is about 0.05% and the uranium content per square meter is 5 kg / m 2 In the mining area, the uranium concentration is generally 20 to 80 mg / L.
[0039] In the present invention, the leaching preparation is preferably further included before the initial leaching; the leaching preparation is preferably: using a leaching preparation agent to dredge the ore layer to obtain a leaching solution; the leaching preparation agent includes CO2 and water; the leaching preparation is preferably carried out by using HCO3 in the leaching solution. - The treatment ends when the concentration reaches 600 mg / L.
[0040] In the present invention, the concentration of CO2 in the leaching preparation agent is preferably 200-400 mg / L, more preferably 250-350 mg / L, and further preferably 300 mg / L. In the present invention, CO2 is added to pre-dredge the ore layer, and the pH value and HCO3 of the leaching solution are monitored simultaneously. - Concentration and uranium concentration and its changes. Generally, HCO3 in the leaching solution - The concentration gradually increases and the pH value decreases, and the uranium concentration will not increase substantially during the pre-leaching stage.
[0041] In the present invention, the mass ratio of CO2 to carbonate sandstone uranium ore in the leaching preparation agent is preferably 2-5:1000-2000, more preferably 2-3:1000-2000, and further preferably 2:1000.
[0042] In the present invention, the leaching preparation preferably also includes geological zoning. The present invention finds out the carbonate content, uranium mineral content and occurrence form of the sandstone uranium ore and the hydrogeological characteristics of the ore layer (the geological exploration report of the ore deposit can be checked), classifies the geological process type of the ore, neutral to weakly alkaline (pH value is 7.0-8.5), ore layer water HCO3 - Sandstone uranium deposits with a concentration of <500 mg / L and a carbonate content in the ore rock (calculated as CO2>1.5%) are classified as carbonate sandstone uranium deposits.
[0043] In the present invention, during the peak leaching period, the concentration of CO2 in the first leaching agent is preferably 600-800 mg / L, more preferably 650-750 mg / L, and further preferably 700 mg / L, and the concentration of O2 is preferably 150-300 mg / L, more preferably 200-270 mg / L, and further preferably 240-250 mg / L.
[0044] In the present invention, during the leaching peak period, the mass ratio of the first leaching agent to the carbonate sandstone uranium ore is preferably 10-20:1000-2000, more preferably 10-15:1000-2000, and further preferably 10:1000.
[0045] In the present invention, a relatively high concentration of CO2 and O2 is added during the peak period of leaching, and the pH value and HCO3 of the leaching solution are monitored simultaneously. - concentration and uranium concentration and their changes; during this period, HCO3 in the leaching solution - The maximum value that the mining area can provide (generally 1000-2000 mg / L) is reached, the pH value is basically maintained between 6.5 and 7.5, and the uranium concentration reaches the peak value of the mining area's entire life leaching (30-150 mg / L). In the first leaching stage, the mining area leaching rate is generally 30%-45%, and the main chemical reactions involved are shown in Formulas 1 to 3:
[0046] CO2+H2O+CaCO3→Ca 2+ +2HCO3 - (Formula 1);
[0047] UO2+0.5O2+2HCO3 - →UO2(CO3)2 2- +H2O (Formula 2);
[0048] UO3+2HCO3 - →UO2(CO3)2 2- +H2O(Formula 3).
[0049] After the first leaching, the present invention uses a second leaching agent to perform a second leaching on the carbonate sandstone uranium ore after the first leaching to obtain a leaching solution, wherein HCO3 - The concentration is not less than 800 mg / L. In the present invention, the second leaching preferably includes the middle leaching and the middle and late leaching carried out in sequence; the second leaching is preferably a flow leaching. In the present invention, when the second leaching agent is added, HCO3 in the leaching solution - When the concentration increment is less than 300-400 mg / L, it enters the middle and late stages of leaching from the middle stage.
[0050] In the present invention, in the middle stage of leaching, the concentration of CO2 in the second leaching agent is preferably 400-600 mg / L, more preferably 450-550 mg / L, and further preferably 500 mg / L, the concentration of O2 is preferably 100-200 mg / L, more preferably 120-180 mg / L, and further preferably 140-160 mg / L, and the concentration of bicarbonate is preferably based on the concentration of HCO3 in the second leaching agent. -The concentration is above 1000 mg / L. In a specific embodiment of the present invention, the concentration of bicarbonate in the second leaching agent is more preferably 200-300 mg / L, and further preferably 240-270 mg / L. At this stage, the carbonate minerals in the sandstone layer have not been completely consumed, but the content is relatively low. The added CO2 reacts with it and can supplement part of the bicarbonate, but the concentration is not enough. Therefore, the present invention supplements bicarbonate to reach the target concentration.
[0051] In the present invention, in the middle stage of leaching, the mass ratio of the second leaching agent to the carbonate sandstone uranium ore is preferably 5-10:1000-2000, more preferably 5-8:1000-2000, and further preferably 5:1000.
[0052] The present invention simultaneously monitors the pH value and HCO3 in the leaching solution in the middle stage of leaching. - concentration and uranium concentration and its changes; during this period, the uranium concentration slowly decreased, and the HCO3 in the leaching solution - It shows a very strong correlation with uranium concentration, and the downward trend is consistent with the downward trend of uranium concentration.
[0053] In the present invention, in the middle and late stages of leaching, the concentration of CO2 in the second leaching agent is preferably 300-400 mg / L, more preferably 320-380 mg / L, and further preferably 340-360 mg / L. The concentration of O2 is preferably 100-200 mg / L, more preferably 120-180 mg / L, and further preferably 140-160 mg / L. The concentration of bicarbonate is preferably based on the concentration of HCO3 in the second leaching agent. - The concentration of bicarbonate is preferably 800-1200 mg / L; in a specific embodiment of the present invention, the concentration of bicarbonate is more preferably 300-500 mg / L, and further preferably 350-450 mg / L. The present invention adds a second leaching agent (CO2) to react with carbonate in carbonate sandstone uranium ore to generate bicarbonate, thereby obtaining a leachate; when HCO3 in the leachate is - When the concentration is 200-300 mg / L, it enters the transformation preparation stage.
[0054] In the present invention, in the middle and late stages of leaching, the mass ratio of the second leaching agent to the carbonate sandstone uranium ore is preferably 3-5:1000-2000, more preferably 3-4:1000-2000, and further preferably 3:1000.
[0055] The present invention simultaneously monitors the pH value and HCO3 of the leaching solution in the middle and late stages of leaching. - Concentration and uranium concentration and their changes. During this period, as the HCO3 in the leaching agent -The decrease trend of uranium concentration slows down if HCO3 is added. - The concentration after leaching exceeds that in the middle stage of leaching, and the uranium concentration will rise slightly, but it cannot be maintained for a long time. The main chemical reaction in the second leaching stage is the same as that in the first leaching stage. In this leaching stage, the leaching rate of the mining area increases by about 15-20%, and the cumulative leaching rate can reach 45%-65%.
[0056] After the second leaching, the present invention uses a transformation preparation leaching agent to perform transformation preparation on the carbonate sandstone uranium ore after the second leaching (obtaining a leachate), and then uses a transformation leaching agent to perform transformation leaching on the carbonate sandstone uranium ore after the transformation preparation to obtain a leachate until the pH value of the leachate is reduced to 2.
[0057] In the present invention, the transformation preparation leachate includes a transformation preparation oxidant and water; the transformation preparation oxidant includes one or both of oxygen and hydrogen peroxide; the concentration of the transformation preparation oxidant in the transformation preparation leachate is preferably 100-200 mg / L, more preferably 120-180 mg / L, and further preferably 140-160 mg / L. - The concentration of uranium decreased significantly (to 500-800 mg / L), and the downward trend of uranium concentration also increased.
[0058] In the present invention, the leaching method for the transformation preparation is preferably flow leaching; the flow rate of the flow leaching is preferably 3 to 10 m 3 / h, more preferably 4 to 8m 3 / h, more preferably 5 to 6 m 3 When the HCO3 concentration in the leaching solution obtained from the transformation preparation reaches 300-400 mg / L, the transformation preparation is completed.
[0059] In the present invention, the concentration of the inorganic acid in the transition leaching agent is preferably 2-3 g / L, more preferably 2.4-2.7 g / L; the inorganic acid preferably includes one or more of sulfuric acid, hydrochloric acid and citric acid.
[0060] In the present invention, the leaching method of the transition leaching is preferably flow leaching; the flow rate of the flow leaching is preferably 3 to 10 m 3 / h, more preferably 4 to 8m 3 / h, more preferably 5 to 6 m 3 / h.
[0061] The present invention simultaneously monitors the pH value and HCO3 of the leaching solution during the transition leaching period. - 、SO4 2- , H + , Ca 2+During this period, the pH value dropped rapidly from 6.5-7.5 to 2-3, and the complex form of leached uranium also changed from uranyl carbonate to uranyl sulfate (specifically, Figure 2 As shown in the figure, the uranium concentration is kept at a low level, generally below 20 mg / L. The main function of this stage is to complete the transformation of the leaching process in the mining area. Due to the relatively short time, the leaching rate in the mining area is increased by about 3% to 5%. The main chemical reactions involved are shown in equations 4 to 7:
[0062] H2SO4+HCO3 - →CO2↑+H2O+SO4 2- (Formula 4);
[0063] H2SO4+CaCO3→Ca 2+ +SO4 2- +CO2↑+H2O (Formula 5);
[0064] UO3+4H + +2SO4 2- →UO2(SO4)2 2- +2H2O (Formula 6);
[0065] Fe2O3+6H + →2Fe 3+ +3H2O (Formula 7).
[0066] After the transformation leaching, the present invention uses a third leaching agent to perform a third leaching on the carbonate sandstone uranium ore after the transformation leaching. In the present invention, the third leaching is the end of the leaching; the concentration of H2SO4 in the third leaching agent is preferably 6-10g / L, more preferably 7-9g / L, and further preferably 8g / L, and the concentration of H2O2 is preferably 0.2-0.5g / L, more preferably 0.3-0.4g / L, and further preferably 0.35g / L.
[0067] In the present invention, the leaching method of the third leaching is preferably flow leaching; the flow rate of the flow leaching is preferably 2 to 8 m 3 / h, more preferably 3 to 7m 3 / h, more preferably 4 to 6 m 3 / h.
[0068] The present invention simultaneously monitors the H in the leaching solution at the end of leaching. + , Ca 2+ , Fe 2+ , Fe 3+ 、SO4 2- and uranium concentrations, H + , Ca 2+ , Fe 2+, Fe 3+ and SO4 2- The concentration of plasma rises rapidly, and the concentration of uranium is higher than that of the previous stage, generally 10-40 mg / L, the leaching rate of the mining area increases by about 15-40%, and the cumulative leaching rate of the mining area is 80-110% (including off-surface ore). In the third leaching stage, in addition to the three chemical reactions of formula 1 to formula 3, the following chemical reactions are also included:
[0069] FeS2+5O2+4H + →Fe 3+ +2H2O+2SO4 2- (Formula 8);
[0070] Fe 3+ +UO2+2SO4 2- →UO2(SO4)2 2- +Fe 2+ (Formula 9);
[0071] UO2+H2O2→UO3+H2O (Equation 10);
[0072] UO2+4H + →U 4+ +2H2O (Formula 11).
[0073] In the present invention, the third leaching preferably also includes a mining area decommissioning stage;
[0074] The decommissioning stage of the mining area is preferably: natural purification after in-situ remediation by microorganisms; the natural purification is preferably started when the pH value of the groundwater in the ore-bearing layer is restored to 5-6. The present invention avoids the direct and violent reaction of carbonate sandstone uranium ore with sulfuric acid to generate a large amount of calcium sulfate precipitation, thereby clogging the ore layer through staged leaching. The present invention improves the leaching rate and production efficiency, and has good economic and ecological benefits.
[0075] The time of each leaching stage or transition leaching period of the present invention is determined according to the specific geological conditions of the ore deposit and the leaching operation conditions. The control node is mainly based on the HCO3 in the leaching solution. - In the present invention, the preparatory period for leaching is generally the 1st to 3rd month, the initial period of leaching is generally the 4th to 12th month, the peak period of leaching is generally the 13th to 36th month, the middle period of leaching is generally the 36th to 60th month, the middle and late period of leaching is generally the 61st to 72nd month, the preparatory period for transformation is generally the 73rd to 75th month, the transformation period is generally the 75th to 78th month, and the final period of leaching is generally the 79th to 96th month.
[0076] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.
[0077] Example 1
[0078] (1) A sandstone uranium ore sample from the Ordos Basin in Inner Mongolia was taken, crushed to a natural particle size, and mixed evenly. The average grade of the sample was 0.0678%, and the average carbonate content (measured in CO2) was 3.38%. The pressure column leaching was used, with a sample length of 1 m, an inner diameter of 40 mm, and a sample density as close to that of the ore deposit as possible (1.8 kg / dm 3 ), the sample weight of each column is 2.6kg; 200L of ore layer water is taken to prepare the leaching agent;
[0079] (2) During the preparatory period for leaching, CO2 was added at a concentration of 200-400 mg / L to pre-clear the ore layer, and the pH value and HCO3 of the leaching solution were monitored simultaneously. - and changes in uranium concentration;
[0080] (3) CO2 and O2 are dissolved in the ore layer water. At the initial stage of leaching, the CO2 concentration is 400-600 mg / L and the O2 concentration is 100-200 mg / L. When the HCO3 concentration in the leachate increases to 800 mg / L, the leaching peak period begins, and the CO2 concentration is 600-800 mg / L and the O2 concentration is 150-300 mg / L. The leachate is injected into a columnar test device under pressure (0.8-1.2 MPa) and a sampling port is set at the top. Samples are taken three times at 6h, 12h and 24h every day to measure the pH value, U concentration and HCO3 of the leachate. - Concentration and SO4 2- Concentration; When the HCO3 in the leaching solution - When the concentration drops from a high value to 800 mg / L, the peak leaching period ends (the first leaching also ends);
[0081] (4) Entering the second leaching stage, the CO2 concentration is 300-400 mg / L, the O2 concentration is 100-200 mg / L, and an NH4HCO3 solution with a concentration of 1000 mg / L is prepared to adjust the HCO3 in the leaching agent. - concentration, ensuring HCO3 in the leaching agent - When the concentration is above 1000mg / L, the pH value and HCO3 of the leaching solution are monitored simultaneously. - and the change of uranium concentration; when the second leaching agent is added to the leaching solution, HCO3 - When the concentration increment is less than 300 mg / L, it enters the middle and late stages of leaching from the middle stage of leaching;
[0082] (5) When HCO3 in the leaching solution -When the concentration is 200-300 mg / L, it enters the transition preparation stage, stops adding CO2 and NH4HCO3, and only adds O2 at a concentration of 100-200 mg / L;
[0083] (6) When the HCO3 concentration in the leachate obtained by the transformation preparation reaches 300-400 mg / L, the transformation preparation is completed, and the transformation leaching stage begins. H2SO4 with a concentration of 2-3 g / L is added, and the pH value and HCO3 of the leachate are monitored simultaneously. - 、SO4 2- , H + , Ca 2+ and uranium concentration changes until the pH value of the leaching solution decreases to 2;
[0084] (7) Entering the third leaching stage, H2SO4 and H2O2 are added, the H2SO4 concentration is 6-10 g / L, the H2O2 concentration is 0.2-0.5 g / L, and the H2O2 concentration of the leaching solution is monitored simultaneously. + , Ca 2+ , Fe 2+ , Fe 3+ 、SO4 2- When the uranium concentration in the leaching solution sample is lower than 3 mg / L, the leaching is stopped. The concentration changes of uranium, bicarbonate and sulfate ions in the leaching solution at different stages, the concentration of uranium and the cumulative leaching rate are shown in Figure 2. Figure 3 and Figure 4 shown.
[0085] according to Figure 3 and Figure 4 It can be seen that: ① In the first leaching stage, carbonate minerals are dissolved by CO2 in a relatively short time, and the HCO3 in the leaching solution - Rapid growth, simultaneous dissolution and complex leaching of uranium minerals; uranium concentration and HCO3 in the leaching solution - The concentration showed a strong positive correlation; the carbonate dissolution rate was fast, and it slowly declined after the peak value, and the uranium concentration in the leaching solution decreased simultaneously;
[0086] ② In the second leaching stage, by adding HCO3 - , maintain the HCO3 of the leaching agent - When the concentration was between 1000 and 1200 mg / L, the uranium concentration rose slightly, and then the downward trend slowed down;
[0087] ③Add 300~500mg / L HCO3 - If it still cannot maintain 1000 mg / L, transformation preparation and transformation leaching can be carried out, and the carbonate content in the ore rock has reached the acid leaching process permit;
[0088] ④ In the third leaching stage, after adding H2SO4 and H2O2, the uranium concentration rebounded rapidly from 12-13 mg / L to more than 30 mg / L, which accelerated the leaching of uranium and maintained above 15 mg / L for a long time. The leaching rate of uranium ore was greatly improved, which was more than 25% higher than that in the second stage.
[0089] Example 2
[0090] The method for recovering carbonate sandstone uranium ore provided in this embodiment is the same as that in Example 1, except that the bicarbonate used in step (4) is replaced by NaHCO3.
[0091] Example 3
[0092] The method for recovering carbonate sandstone uranium ore provided in this embodiment is the same as that in Example 1, except that the bicarbonate used in step (4) is replaced by KHCO3.
[0093] Example 4
[0094] The method for recovering carbonate sandstone uranium ore provided in this embodiment is the same as that in Example 1, with the only difference being that the bicarbonate used in step (4) is replaced by Mg(HCO3)2.
[0095] Example 5
[0096] The method for recovering carbonate sandstone uranium ore provided in this embodiment is the same as that in Example 1, except that the O2 used in step (5) is replaced by hydrogen peroxide.
[0097] Example 6
[0098] The method for recovering carbonate sandstone uranium ore provided in this embodiment is the same as that in Example 1, except that the H2SO4 used in step (6) is replaced by hydrochloric acid.
[0099] It can be seen from the above embodiments that the recovery method of carbonate sandstone uranium ore provided by the present invention increases the leaching rate by more than 15%, has high leaching rate and high efficiency.
[0100] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for recovering carbonate sandstone uranium ore, characterized in that: The following steps are involved: (1) Using a first leaching agent to perform a first leaching on a carbonate sandstone uranium ore to obtain a leaching solution until HCO3 in the leaching solution is - The concentration of is reduced to 800 mg / L; the first leaching agent includes CO2, O2 and water; (2) using a second leaching agent to perform a second leaching on the carbonate sandstone uranium ore after the first leaching to obtain a leachate, wherein HCO3 - The concentration is not less than 800 mg / L; the second leaching agent includes CO2, O2, water and bicarbonate; the bicarbonate includes one or more of NaHCO3, NH4HCO3, KHCO3 and Mg(HCO3)2; (3) after the carbonate sandstone uranium ore after the second leaching is subjected to transformation preparation using a transformation preparation leaching agent, the carbonate sandstone uranium ore after the transformation preparation is subjected to transformation leaching using a transformation preparation leaching agent to obtain a leachate until the pH value of the leachate is reduced to 2; the transformation preparation leaching agent comprises a transformation preparation oxidant and water; the transformation preparation oxidant comprises one or two of oxygen and hydrogen peroxide; the transformation leaching agent comprises an inorganic acid and water; (4) performing a third leaching on the carbonate sandstone uranium ore after the transition leaching using a third leaching agent; the third leaching agent comprises H2SO4, H2O2 and water.
2. The recycling method according to claim 1, characterized in that: The first leaching includes an initial leaching period and a peak leaching period performed sequentially; In the initial stage of leaching, the concentration of CO2 in the first leaching agent is 400-600 mg / L, and the concentration of O2 is 100-200 mg / L.
3. The recycling method according to claim 2, characterized in that: During the peak leaching period, the concentration of CO2 in the first leaching agent is 600-800 mg / L, and the concentration of O2 is 150-300 mg / L.
4. The recycling method according to claim 1, characterized in that: The initial stage of leaching also includes leaching preparation; The leaching preparation is: using a leaching preparation agent to dredge the ore layer; the leaching preparation agent includes CO2 and water.
5. The recycling method according to claim 4, characterized in that: The concentration of CO2 in the leaching preparation agent is 200-400 mg / L.
6. The recycling method according to claim 1, characterized in that: The second leaching includes a mid-leaching phase and a mid-late-leaching phase performed sequentially; In the middle stage of leaching, the concentration of CO2 in the second leaching agent is 400-600 mg / L, the concentration of O2 is 100-200 mg / L, and the concentration of bicarbonate is based on the concentration of HCO3 in the second leaching agent. - The concentration is above 1000mg / L.
7. The recycling method according to claim 6, characterized in that: In the middle and late stages of leaching, the concentration of CO2 in the second leaching agent is 300-400 mg / L, the concentration of O2 is 100-200 mg / L, and the concentration of bicarbonate is based on the concentration of HCO3 in the leaching agent. - The concentration is 800-1200 mg / L.
8. The recycling method according to claim 1, characterized in that: The concentration of the transformation preliminary oxidant in the transformation preliminary leaching agent is 100-200 mg / L.
9. The recycling method according to claim 1, characterized in that: The concentration of the inorganic acid in the transition leaching agent is 2-3 g / L.
10. The recycling method according to claim 1, characterized in that: The concentration of H2SO4 in the third leaching agent is 6-10 g / L, and the concentration of H2O2 is 0.2-0.5 g / L.
Citation Information
Patent Citations
Desalination little-reagent ground-dipping uranium extraction method
CN101429860A
Microreagent neutral in-situ leaching process for uranium recovery
CN106507823B
Method for in-situ leaching of uranium from sandstone-type uranium deposits
CN111455173A
Multi-reagent combined well washing method for CO2+O2 in-situ leaching uranium mining mine
CN114369732A
Neutral in-situ leaching uranium mining method and system
CN115725837A
Cited By
Method for constructing artificial water-resisting layer in carbon dioxide and oxygen in-situ leaching exploitation of high-carbonate sandstone uranium deposit