Silver-based core-shell conductive film applied to transparent heater and preparation method of silver-based core-shell conductive film
The preparation of silver-based core-shell conductive films through electrospinning and magnetron sputtering technology solves the problem of low heating efficiency of traditional transparent heaters under high transmittance and low voltage, and achieves the effect of efficient heating at low voltage.
Patent Information
- Application Number
- CN202411001278.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional transparent heaters are difficult to achieve high visible light transmittance and low operating voltage at the same time, resulting in high energy loss and low heating efficiency.
Electrospinning technology is used to prepare fiber wires with high aspect ratio, and a silver-based core-shell structure is formed through magnetron sputtering technology, which increases the contact tightness and adhesion between nanowires, and adjusts the thickness of the oxide protective layer to optimize Transmittance and square resistance form a silver-based core-shell conductive film.
The temperature can reach 40℃ at 1V voltage and heat to about 100℃ at 2V voltage, achieving low voltage and efficient heating, suitable for application scenarios such as vehicle glass, lidar windows and camera windows.
Smart Images

Figure CN118880261A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive film preparation, and in particular to a silver-based core-shell conductive film applied to a transparent heater and a preparation method thereof. Background Art
[0002] Transparent heaters are widely used in the fields of smart window defogger and deicer, thermochromic, automobile rearview mirror defogger, lidar window heating, camera window heating, etc. due to their high heating efficiency and high light transmittance. Traditional transparent conductive films such as indium tin oxide (ITO), aluminum-doped zinc oxide (AZO), and fluorine-doped tin oxide (FTO) cannot achieve high visible light transmittance and low square resistance at the same time, which further limits their application in transparent heaters. Silver nanowires have lower square resistance and higher visible light transmittance, making them an effective candidate material for making transparent heaters. However, the current transparent heaters based on silver nanowires have a high heating voltage and cannot achieve efficient heating at low operating voltages, which means that the transparent heater has a high energy loss during operation. The reason is that the prepared silver nanowires have a large square resistance and part of the electrical energy cannot be effectively converted into thermal energy. According to Joule's law, the heat generated by the current passing through the conductor per unit time is Q=U 2 / R, so at the same voltage, the lower the sheet resistance, the more heat it generates, that is, the higher the heating efficiency of the transparent heater. However, the reduction of sheet resistance will inevitably reduce the visible light transmittance. Therefore, it is difficult for existing transparent heaters to achieve high transmittance and low operating voltage at the same time. Summary of the invention
[0003] The purpose of the present invention is to provide a silver-based core-shell conductive film for use in a transparent heater and a preparation method thereof, which can solve the problem in the prior art that transparent heaters are difficult to achieve both high transmittance and low operating voltage.
[0004] The objective of the present invention is achieved through the following technical solutions: In a first aspect, the present invention provides a method for preparing a silver-based core-shell conductive film for a transparent heater, comprising the following steps: Step 1, injecting the prepared spinning solution into a syringe, and connecting the syringe to a catheter and an injection needle in sequence, wherein the injection needle is connected to the positive electrode of a high-voltage transformer; Step 2, fix the cleaned transparent substrate on the electrospinning roller; make the roller rotate at a set speed, connect the roller to the negative pole of the high-voltage transformer, and turn on the heating device above the roller; Step 3, injecting the spinning solution from the syringe into the catheter; turning on the high-voltage transformer button to allow the droplets at the injection needle to be ejected quickly to form a charged jet; finally, under the action of the electrostatic field, the fiber is stretched and solidified to form a fiber filament, which is deposited on a transparent substrate; Step 4: placing the transparent substrate with the fiber filaments deposited thereon into a magnetron sputtering device, and sputtering in sequence to form a silver layer and an oxide protective layer to form a silver-based core-shell structure transparent conductive film; the thickness of the silver layer is 250nm~340nm, and the thickness of the oxide protective layer is 10nm~225nm.
[0005] Furthermore, the spinning solution is a polyvinyl alcohol solution or a polyvinylidene fluoride solution; the solvent in the polyvinyl alcohol solution is deionized water, and the solvent mass accounts for 8wt%~15wt%; the solvent in the polyvinylidene fluoride solution is N,N-dimethylformamide and acetone, the ratio of N,N-dimethylformamide and acetone is 7:3 or 6:4, and the solvent mass accounts for 10wt%~20wt%.
[0006] Furthermore, the oxide protective layer is one of a zinc oxide protective layer, an aluminum oxide protective layer, a tin oxide protective layer, and a silicon oxide protective layer.
[0007] Furthermore, in step 2, the rotation speed of the drum is 100 r / min~300 r / min; the heating device controls the heating temperature between 30°C~55°C.
[0008] Furthermore, in step 3, the spinning solution is injected into the catheter from the syringe at a speed of 0.05 ml / min to 0.15 ml / min.
[0009] Furthermore, in step 3, the output voltage of the high-voltage transformer is controlled between 15 kV and 20 kV.
[0010] Furthermore, in step 3, the fiber filaments are deposited on the transparent substrate for a period of 18 to 22 minutes.
[0011] In a second aspect, the present invention provides a silver-based core-shell conductive film for use in a transparent heater, which is prepared using the above-mentioned preparation method and includes a fiber layer, a silver layer and an oxide protective layer sequentially prepared on a transparent substrate.
[0012] Furthermore, the oxide protective layer is one of a zinc oxide protective layer, an aluminum oxide protective layer, a tin oxide protective layer, and a silicon oxide protective layer.
[0013] In a third aspect, the present invention provides a transparent heater, wherein electrodes are prepared on the above-mentioned silver-based core-shell conductive film by ion sputtering or screen printing, and connected to an external power source by a wire to form a transparent heater.
[0014] The silver-based core-shell conductive film and preparation method thereof for transparent heaters of the present invention utilize electrostatic spinning technology to obtain fiber filaments with a high aspect ratio, and then utilize magnetron sputtering technology to sputter Ag film (silver film), thereby obtaining Ag nanowires (silver nanowires) with a high aspect ratio. On this basis, a layer of oxide is sputtered onto the surface of the Ag nanowires to make the contact between the Ag nanowires closer, and also increase the adhesion of the Ag nanowires to the substrate. Finally, by adjusting the thickness of the oxide, the transmittance of the Ag nanowires in the visible light range is above 75% (including the substrate), and the square resistance is below 1 ohm. The temperature of the heater prepared in this way can rise to 40°C at a voltage of 1V, and can be heated to about 100°C at a low voltage of 2V. The above results show that the prepared transparent heater has good performance and is expected to be used in various application scenarios such as vehicle glass heating, lidar window heating, and camera window heating. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 A schematic diagram of the transmittance variation trend of the transparent conductive film at different aluminum oxide thicknesses according to Example 1 of the present invention; Figure 2 This is a schematic diagram of the change trend of the square resistance of the transparent conductive film under different aluminum oxide thicknesses according to the first embodiment of the invention; Figure 3 The heating temperatures of the transparent heater prepared in Example 1 of the present invention at different voltages; Figure 4 The cycle test results of the heater prepared in Example 1 of the present invention at a voltage of 2V; Figure 5 The long-term heating result of the heater prepared in Example 1 of the present invention at a voltage of 2V; Figure 6 It is a schematic diagram of the steps of the method for preparing the silver-based core-shell conductive film of the present invention. DETAILED DESCRIPTION
[0016] The embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.
[0017] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the contents disclosed in this specification. Obviously, the described embodiments are only a part of the embodiments of the present disclosure, rather than all of the embodiments. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present disclosure. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present disclosure.
[0018] Embodiment 1 A method for preparing a silver-based core-shell conductive film for a transparent heater comprises the following steps: Step 1: Inject the prepared spinning solution into a syringe, and connect the syringe to a catheter and an injection needle in sequence, wherein the injection needle is connected to the positive pole of a high-voltage transformer.
[0019] The spinning solution is a polyvinyl alcohol (PVA) solution, wherein the solvent in the PVA solution is deionized water, and the mass percentage is 8wt% to 15wt%.
[0020] Step 2: Fix the cleaned transparent substrate on the electrospinning drum; make the drum rotate at a certain speed, the speed is 100r / min; at the same time, connect the drum to the negative pole of the high-voltage transformer, and turn on the heating device above the drum, and control the heating temperature at 55°C to dry the spinning and shape it.
[0021] Furthermore, the transparent substrate is one of sodium lime glass, high aluminum glass, high borosilicate glass and quartz glass.
[0022] Step 3: Inject the spinning solution from the syringe into the catheter at a rate of 0.10 ml / min; turn on the high-voltage transformer button and control the voltage at 20 kV, so that the conical droplets at the injection needle are ejected quickly to form a charged jet. Finally, under the action of the electrostatic field, it is stretched and solidified to form a fiber layer, which is deposited on a transparent substrate. The collection time of the fiber is 20 minutes.
[0023] Step 4: Place the transparent substrate with the fiber filaments deposited thereon into a magnetron sputtering device, and sequentially sputter to form a silver layer and an aluminum oxide protective layer, thereby forming a silver-based core-shell structure transparent conductive film, wherein the thickness of the silver layer is 280 nm and the thickness of the aluminum oxide protective layer is 135 nm.
[0024] Furthermore, the aluminum oxide protective layer is formed by sputtering an aluminum oxide target material. The aluminum oxide protective layer can also be replaced by an aluminum oxide protective layer, a tin oxide protective layer or a silicon oxide protective layer, each of which is prepared by a corresponding oxide target material.
[0025] The purity of the metal silver target and the oxide target is greater than 99.99%. The metal silver target, oxide target and glass used in the present invention are all commercially available products. The silver-based core-shell conductive film used in a transparent heater is prepared by the above method, and comprises a fiber layer, a silver layer and an oxide protective layer which are sequentially prepared on a transparent substrate.
[0026] Furthermore, the oxide protective layer is an aluminum oxide protective layer.
[0027] A transparent heater is formed by preparing a rectangular electrode on a silver-based core-shell conductive film by ion sputtering and connecting it to an external power source by a wire.
[0028] The present invention uses a high aspect ratio fiber prepared by electrospinning as a template, and uses magnetron sputtering technology to sputter an Ag film and an oxide protective layer in sequence, thereby obtaining a high aspect ratio Ag-based core pit structure nanowire. The sputtered oxide protective layer has four functions: ① increasing the adhesion between the nanowire and the substrate; ② making the contact between the nanowires closer, thereby increasing the conductivity; ③ delaying the oxidation of Ag in normal operation; ④ using the difference in the refractive index and absorption coefficient between the oxide and Ag to further enhance the transmittance through the interference effect. Finally, by adjusting the thickness of the oxide, a transparent conductive film with a transmittance of more than 75% (including the substrate) and a square resistance of less than 1 ohm in the visible light range can be prepared. The heater prepared on this basis can rise to 40°C at a voltage of 1V, and can be heated to about 100°C at a low voltage of 2V. The above results show that the prepared transparent heater has good performance and is expected to be used in various application scenarios such as vehicle glass heating, lidar window heating, and camera window heating.
[0029] Figure 1 Schematic diagram of the transmittance variation trend of transparent conductive films under different aluminum oxide thicknesses. Figure 2 Schematic diagram of the change trend of the square resistance of transparent conductive films under different aluminum oxide thicknesses. Figure 1 It can be seen that when the thickness of aluminum oxide is 135nm, its average transmittance is the highest, which is 77%. Figure 2It shows that as the thickness of aluminum oxide increases from 45nm to 135nm, the square resistance of the silver-based core-shell structure transparent conductive film shows a gradual downward trend. The reason may be that as the thickness of aluminum oxide increases, the contact between the nanowires becomes closer, thereby reducing the junction resistance between the nanowires and causing the square resistance to decrease. When the thickness of aluminum oxide is greater than 135nm, the film quality of aluminum oxide is better and the resistance increases, so the square resistance of the silver-based core-shell structure transparent conductive film begins to increase. Figure 1 and Figure 2 The results show that the transmittance and square resistance of the silver-based core-shell structure transparent conductive film are affected by the thickness of aluminum oxide. When the thickness is 135nm, the square resistance is the smallest and the transmittance is the largest. Based on this, a rectangular electrode was prepared on the silver-based core-shell structure transparent conductive film by small ion sputtering to test the heating performance of the transparent heater.
[0030] Figure 3 The heating temperature of the prepared transparent heater under different voltages shows that the temperature can rise to 42°C at a voltage of 1V, can be heated to about 100°C at a low voltage of 2V, and can be heated to above 120°C at a low voltage of 3V.
[0031] Figure 4 The prepared transparent heater was subjected to a switching cycle test at a voltage of 2V. After multiple cycles, its maximum heating temperature did not decay significantly.
[0032] Figure 5 This is the test result diagram of the prepared transparent heater working for a long time at a voltage of 2V, and its maximum temperature does not show obvious decay.
[0033] The above results show that the prepared transparent heater has good heating performance and can be heated to 42°C at a low voltage of 1V. It also has good stability in cycle tests and long-term work. It is expected to be used in various application scenarios such as vehicle glass heating, lidar window heating, and camera window heating.
[0034] Embodiment 2 A method for preparing a silver-based core-shell conductive film for a transparent heater comprises the following steps: Step 1: Inject the prepared spinning solution into a syringe, and connect the syringe to a catheter and an injection needle in sequence, wherein the injection needle is connected to the positive pole of a high-voltage transformer.
[0035] The spinning solution is a polyvinylidene fluoride (PVDF) solution. The solvent in the PVDF solution is DMF (N,N-dimethylformamide) and acetone, the ratio is 7:3 or 6:4, and the mass percentage of PVDF is 10wt%~20wt%.
[0036] Step 2: Fix the cleaned transparent substrate on the electrospinning drum; make the drum rotate at a certain speed, the speed is 200r / min; at the same time, connect the drum to the negative pole of the high-voltage transformer, and turn on the heating device above the drum, and control the heating temperature at 30°C to dry the spinning and make it fixed.
[0037] Furthermore, the transparent substrate is one of sodium lime glass, high aluminum glass, high borosilicate glass and quartz glass.
[0038] Step 3: Inject the spinning solution from the syringe into the catheter at a rate of 0.05 ml / min; turn on the high-voltage transformer button and control the voltage at 15 kV, so that the conical droplets at the injection needle are ejected quickly to form a charged jet. Finally, under the action of the electrostatic field, it is stretched and solidified to form a fiber layer, which is deposited on a transparent substrate. The collection time of the fiber is 22 minutes.
[0039] Step 4: Place the transparent substrate with the fiber filaments deposited thereon into a magnetron sputtering device, and sequentially sputter to form a silver layer and a zinc oxide protective layer, thereby forming a silver-based core-shell structure transparent conductive film, wherein the thickness of the silver layer is 250 nm and the thickness of the zinc oxide is 10 nm.
[0040] Furthermore, the zinc oxide protective layer is formed by sputtering a zinc oxide target.
[0041] The purity of metallic silver target and zinc oxide target is both >99.99%. The silver-based core-shell conductive film used in a transparent heater is prepared by the above method, and comprises a fiber layer, a silver layer and an oxide protective layer which are sequentially prepared on a transparent substrate.
[0042] Furthermore, the oxide protective layer is a zinc oxide protective layer.
[0043] A transparent heater is formed by preparing rectangular electrodes on a silver-based core-shell conductive film by screen printing and connecting them to an external power source by a wire.
[0044] The experiment shows that the transparent heater of this embodiment has a square resistance of 390mΩ, an average light transmittance of 75%, and a temperature that can rise to 40°C at a voltage of 1V.
[0045] Embodiment 3 A method for preparing a silver-based core-shell conductive film for a transparent heater comprises the following steps: Step 1: Inject the prepared spinning solution into a syringe, and connect the syringe to a catheter and an injection needle in sequence, wherein the injection needle is connected to the positive pole of a high-voltage transformer.
[0046] The spinning solution is a polyvinylidene fluoride (PVDF) solution. The solvent in the PVDF solution is DMF (N,N-dimethylformamide) and acetone, the ratio is 7:3 or 6:4, and the mass percentage of PVDF is 10wt%~20wt%.
[0047] Step 2: Fix the cleaned transparent substrate on the electrospinning drum; make the drum rotate at a certain speed, the speed is 300r / min; at the same time, connect the drum to the negative pole of the high-voltage transformer, and turn on the heating device above the drum, and control the heating temperature at 40°C to dry the spinning and make it fixed.
[0048] Furthermore, the transparent substrate is one of sodium lime glass, high aluminum glass, high borosilicate glass and quartz glass.
[0049] Step 3: Inject the spinning solution from the syringe into the catheter at a rate of 0.15 ml / min; turn on the high-voltage transformer button and control the voltage at 18 kV, so that the conical droplets at the injection needle are ejected quickly to form a charged jet. Finally, under the action of the electrostatic field, it is stretched and solidified to form a fiber layer, which is deposited on a transparent substrate. The collection time of the fiber is 18 minutes.
[0050] Step 4: Place the transparent substrate with the fiber filaments deposited thereon into a magnetron sputtering device, and sequentially sputter to form a silver layer and a silicon oxide protective layer, thereby forming a silver-based core-shell structure transparent conductive film, wherein the thickness of the silver layer is 320 nm and the thickness of the silicon oxide protective layer is 75 nm.
[0051] Furthermore, the silicon oxide protective layer is formed by sputtering a silicon oxide target.
[0052] The purity of metal silver target and silicon oxide target is both >99.99%. The silver-based core-shell conductive film used in a transparent heater is prepared by the above method, and comprises a fiber layer, a silver layer and an oxide protective layer which are sequentially prepared on a transparent substrate.
[0053] Furthermore, the oxide protective layer is a silicon oxide protective layer.
[0054] A transparent heater is formed by preparing a rectangular electrode on a silver-based core-shell conductive film by ion sputtering and connecting it to an external power source by a wire.
[0055] Experiments have shown that the transparent heater of this embodiment has a square resistance of 410 mΩ, an average light transmittance of 79%, and a temperature that can rise to 40° C. at a voltage of 1 V.
[0056] Embodiment 4 A method for preparing a silver-based core-shell conductive film for a transparent heater comprises the following steps: Step 1: Inject the prepared spinning solution into a syringe, and connect the syringe to a catheter and an injection needle in sequence, wherein the injection needle is connected to the positive pole of a high-voltage transformer.
[0057] The spinning solution is a polyvinylidene fluoride (PVDF) solution. The solvent in the PVDF solution is DMF (N,N-dimethylformamide) and acetone, the ratio is 7:3 or 6:4, and the mass percentage of PVDF is 10wt%~20wt%.
[0058] Step 2: Fix the cleaned transparent substrate on the electrospinning drum; make the drum rotate at a certain speed, the speed is 300r / min; at the same time, connect the drum to the negative pole of the high-voltage transformer, and turn on the heating device above the drum, and control the heating temperature at 40°C to dry the spinning and make it fixed.
[0059] Furthermore, the transparent substrate is one of sodium lime glass, high aluminum glass, high borosilicate glass and quartz glass.
[0060] Step 3: Inject the spinning solution from the syringe into the catheter at a rate of 0.15 ml / min; turn on the high-voltage transformer button and control the voltage at 18 kV, so that the conical droplets at the injection needle are ejected quickly to form a charged jet. Finally, under the action of the electrostatic field, it is stretched and solidified to form a fiber layer, which is deposited on a transparent substrate. The collection time of the fiber is 18 minutes.
[0061] Step 4: Place the transparent substrate with the fiber filaments deposited thereon into a magnetron sputtering device, and sequentially sputter to form a silver layer and a tin oxide protective layer, thereby forming a silver-based core-shell structure transparent conductive film, wherein the thickness of the silver layer is 340 nm and the thickness of the tin oxide protective layer is 225 nm.
[0062] Furthermore, the tin oxide protective layer is formed by sputtering a tin oxide target.
[0063] The purity of metallic silver target and tin oxide target is both >99.99%. The silver-based core-shell conductive film used in a transparent heater is prepared by the above method, and comprises a fiber layer, a silver layer and an oxide protective layer which are sequentially prepared on a transparent substrate.
[0064] Furthermore, the oxide protective layer is a tin oxide protective layer.
[0065] A transparent heater is formed by preparing a rectangular electrode on a silver-based core-shell conductive film by ion sputtering and connecting it to an external power source by a wire.
[0066] Experiments have shown that the transparent heater of this embodiment has a square resistance of 410 mΩ, an average light transmittance of 79%, and a temperature that can rise to 40° C. at a voltage of 1 V.
[0067] The above is only for explaining the implementation mode of the present invention and is not intended to limit the present invention. For those skilled in the art, any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention without creative work should be included in the protection scope of the present invention.
Claims
1. A method for preparing a silver-based core-shell conductive film for a transparent heater, characterized in that: The following steps are involved: Step 1, injecting the prepared spinning solution into a syringe, and connecting the syringe to a catheter and an injection needle in sequence, wherein the injection needle is connected to the positive electrode of a high-voltage transformer; Step 2, fix the cleaned transparent substrate on the roller; make the roller rotate at a set speed, connect the roller to the negative pole of the high-voltage transformer, and turn on the heating device above the roller; Step 3, injecting the spinning solution from the syringe into the catheter; Turn on the high-voltage transformer to make the droplets at the jet needle spray out quickly, forming a charged jet; finally, under the action of the electrostatic field, it is stretched and solidified to form fiber filaments, which are deposited on a transparent substrate; Step 4: placing the transparent substrate with the fiber filaments deposited thereon into a magnetron sputtering device, and sputtering in sequence to form a silver layer and an oxide protective layer to form a silver-based core-shell structure transparent conductive film; the thickness of the silver layer is 250nm~340nm, and the thickness of the oxide protective layer is 10nm~225nm.
2. The method for preparing a silver-based core-shell conductive film for a transparent heater according to claim 1, characterized in that: The spinning solution is a polyvinyl alcohol solution or a polyvinylidene fluoride solution; the solvent in the polyvinyl alcohol solution is deionized water, and the solvent mass accounts for 8wt%~15wt%; the solvent in the polyvinylidene fluoride solution is N,N-dimethylformamide and acetone, the ratio of N,N-dimethylformamide to acetone is 7:3 or 6:4, and the solvent mass accounts for 10wt%~20wt%.
3. The method for preparing a silver-based core-shell conductive film for a transparent heater according to claim 1, characterized in that: The oxide protective layer is one of a zinc oxide protective layer, an aluminum oxide protective layer, a tin oxide protective layer, and a silicon oxide protective layer.
4. The method for preparing a silver-based core-shell conductive film for a transparent heater according to claim 1, characterized in that: In step 2, the rotation speed of the drum is 100 r / min-300 r / min; the heating device controls the heating temperature between 30° C. and 55° C.
5. The method for preparing a silver-based core-shell conductive film for a transparent heater according to claim 1, characterized in that: In the step 3, the spinning solution is injected into the catheter from the syringe at a speed of 0.05 ml / min to 0.15 ml / min.
6. The method for preparing a silver-based core-shell conductive film for a transparent heater according to claim 1, characterized in that: In step 3, the output voltage of the high-voltage transformer is controlled between 15kV and 20kV.
7. The method for preparing a silver-based core-shell conductive film for a transparent heater according to claim 1, characterized in that: In step 3, the fiber filaments are deposited on the transparent substrate for a period of 18 to 22 minutes.
8. A silver-based core-shell conductive film for a transparent heater, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 7, comprising a fiber layer, a silver layer and an oxide protective layer prepared in sequence on a transparent substrate.
9. The silver-based core-shell conductive film according to claim 8, characterized in that: The oxide protective layer is one of a zinc oxide protective layer, an aluminum oxide protective layer, a tin oxide protective layer, and a silicon oxide protective layer.
10. A transparent heater, characterized in that: Electrodes are prepared on the silver-based core-shell conductive film according to claim 8 or 9 by ion sputtering or screen printing, and are connected to an external power source by wires to form a transparent heater.