Material capable of spontaneously growing Ag crystal whiskers and preparation method thereof

By hot-dip plating and diffusing heat treatment on Fe-Cr-B cast steel, the Cr-Al-B MAB phase was generated and corrosion reaction was carried out in AgCl molten salt, and Ag whiskers in Cr-Al-B MAB phase was achieved. The spontaneous growth of the FeAl3 region solves the growth problem of Ag whiskers in the MAX phase and MAB phase, and improves the Ag replacement efficiency and whisker morphology.

CN118880468APending Publication Date: 2024-11-01HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410952859.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art has failed to effectively achieve the growth of Ag whiskers on the MAX phase and MAB phase, especially the replacement of M or A atoms and the self-growth of whiskers by Ag.

Method used

By hot-dipping Fe-Cr-B cast steel with Al-Si alloy and diffusing heat treatment, a Cr-Al-B MAB phase periodic laminate structure coating was generated, and then corrosion reaction was performed in AgCl molten salt to generate Cr-Al -Ag-B MAB phase and Fe-Al-Ag ternary phase lead to substitution and spontaneous growth of Ag atoms.

Benefits of technology

The spontaneous growth of Ag whiskers in the Cr-Al-B MAB phase and FeAl3 region was achieved, forming irregular or prism-shaped Ag whiskers, improving the Ag displacement efficiency and whisker growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880468A_ABST
    Figure CN118880468A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of novel materials and novel material preparation, and particularly relates to a material capable of spontaneously growing Ag whiskers and a preparation method thereof.The preparation method comprises the steps that Fe-Cr-B cast steel Al-Si alloy melt is subjected to hot dipping and subsequent diffusion heat treatment, then the Fe-Cr-B cast steel Al-Si alloy melt is immersed into AgCl molten salt to be corroded, and finally a whitened periodic lamellar structure is obtained, and the whitening Cr-Al-Ag-B MAB phase can be used for spontaneously growing Ag crystal whiskers. According to the method, the Cr-Al-Ag-B MAB phase is generated through a simple process, the precious metal Ag crystal whiskers can spontaneously grow, meanwhile, the variety of the MAB phase is widened, and a new method is provided for growth of the Ag crystal whiskers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new materials, and in particular to a material for spontaneously growing Ag whiskers and a preparation method thereof. Background Art

[0002] Metal whiskers refer to filamentous crystals that grow spontaneously on solid surfaces such as metals. Ag is an inert precious metal, and there are few reports on the spontaneous growth of Ag whiskers. Tohmyoh et al. in Japan found that Ag whiskers can be grown on SiO2 film substrates through complex processes. Chen et al. in Taiwan, China found that Ag whiskers can grow on Ag alloys. MAX phase is a special type of compound with layered atomic arrangement, in which M is a transition metal element, A is a 13-16 group element, and X is a C, N element. The binding force between the A layer atoms in the MAX phase and the adjacent MX layer is weak, and it is very easy to deintercalate. Some scholars have shown that Ag can replace Al and Ti atoms in the Ti2AlC MAX phase at the M and A positions respectively. Some scholars have also found based on first-principles calculations that Ag can preferentially replace Ti atoms in the Ti2AlC MAX phase at the M position, but no Ag whiskers have been found to grow on the MAX phase.

[0003] The MAB phase is similar to the widely-regarded MAX phase (B is boron), but there is no report on the substitution of Ag for the M or A atoms in the MAB phase. The applicant's previous research found that when hot-dip aluminum is applied to Fe-Cr-B cast steel, a periodic lamellar structure (PLS) consisting of alternating FeAl3 and Cr-Al-B MAB phases is generated at the solid-liquid interface. It is still unknown whether Ag will substitute the Cr / Al atoms in the Cr-Al-B MAB phase like it substitutes the M / A atoms in the MAX phase. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a material for spontaneously growing Ag whiskers and a preparation method thereof, and to prepare a periodic lamellar structure coating containing a Cr-Al-Ag-B MAB phase and capable of spontaneously growing noble metal Ag whiskers.

[0005] To solve the above technical problems, the technical solution adopted by the present invention is: a material for spontaneously growing Ag whiskers, comprising a periodic lamellar structure coating, wherein the periodic lamellar structure coating comprises a Cr-Al-B MAB phase containing Ag atoms.

[0006] In a preferred embodiment, the Ag atoms exist in two forms, one is the Ag atoms in the Cr-Al-Ag-B MAB phase, and the other is the single substance Ag in the Cr-Al-Ag-B MAB phase or on the grain boundary of the Cr-Al-B MAB phase.

[0007] In a preferred embodiment, the Ag atoms in the periodic lamellar structure coating spontaneously generate Ag whiskers after being left to stand.

[0008] In a preferred embodiment, the Ag whiskers are irregular or prismatic in shape.

[0009] The present invention also provides a method for preparing a material for spontaneously growing Ag whiskers, comprising the following steps: Step 1: Preparation of periodic layer structure coating: The Fe-Cr-B cast steel is immersed in an Al-Si alloy melt for hot-dip plating. After hot-dip plating, the sample is quickly taken out of the alloy melt, air-cooled, and then subjected to diffusion heat treatment. A periodic lamellar structure coating consisting of alternating Cr-Al-B MAB phases and FeAl3 is formed on the interface of the boride (Cr, Fe)2B / Al melt in the Fe-Cr-B cast steel. Step 2: AgCl molten salt corrosion: The specimen containing the periodic lamellar structure coating prepared in step 1 is immersed in AgCl molten salt for molten salt corrosion. The specimen taken out after the molten salt corrosion is cleaned by ultrasonic wave to remove the residual salt on the surface. The Cr-Al-B MAB phase in the periodic lamellar structure coating after the AgCl molten salt corrosion contains Ag atoms.

[0010] In a preferred embodiment, in step 2, the temperature of the AgCl molten salt is 600-800° C., and the test piece containing the periodic lamellar structure coating is immersed in the AgCl molten salt for corrosion for 5 minutes to 120 minutes.

[0011] In the preferred embodiment, in the step 2, the Ag atoms in the periodic lamellar structure coating after AgCl molten salt corrosion are derived from Ag in the AgCl molten salt. + .

[0012] In a preferred embodiment, in step 2, the chemical reaction between the Cr-Al-B MAB phase in the periodic lamellar structure coating and the AgCl molten salt is: Cr-Al-B MAB phase + AgCl→Cr-Al-Ag-B MAB phase + AlCl3 + Ag.

[0013] In the preferred embodiment, in step 2, the AgCl molten salt preferentially reacts chemically with the Cr-Al-BMAB phase in the periodic lamellar structure coating; as the temperature of the AgCl molten salt increases and the corrosion time prolongs, the FeAl3 in the periodic lamellar structure coating reacts with the AgCl molten salt to generate a Fe-Al-Ag ternary phase.

[0014] In a preferred solution, the elemental Ag in the periodic lamellar structure coating after AgCl molten salt corrosion is discontinuously distributed in the entire Cr-Al-B MAB phase region, and the spontaneously grown Ag whiskers are also discontinuously distributed.

[0015] The present invention provides a material for spontaneously growing Ag whiskers and a preparation method thereof, which have the following beneficial effects: 1. A PLS coating containing alternating FeAl3 and Cr-Al-B MAB phases is obtained by hot-dip plating of Fe-Cr-B cast steel with Al-Si alloy and subsequent diffusion heat treatment. Then, AgCl molten salt immersion corrosion is performed to obtain Cr-Al-B MAB phase replaced by Ag.

[0016] 2. AgCl molten salt reacts with PLS, especially with the Cr-Al-B MAB phase therein to generate a quaternary Cr-Al-Ag-B MAB phase, and also generates Ag element on its grain boundaries.

[0017] 3. With the extension of corrosion time and the increase of molten salt temperature, FeAl3 in PLS will also react with high-temperature AgCl molten salt to generate Fe-Al-Ag ternary phase.

[0018] 4. Ag whiskers will spontaneously grow in the whitish Cr-Al-B MAB phase and FeAl3 phase areas of the PLS coating after corrosion by AlCl molten salt. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The present invention will be further described below in conjunction with the accompanying drawings and embodiments: Figure 1 This is a cross-sectional microstructure diagram of the PLS coating prepared in Example 1 after being corroded by AgCl molten salt; Figure 2 Cr element distribution diagram of the cross section of the PLS coating prepared in Example 1 after being corroded by AgCl molten salt; Figure 3 The Ag element distribution diagram of the cross section of the PLS coating prepared in Example 1 after being corroded by AgCl molten salt; Figure 4 Ag whiskers grown spontaneously in the cross section of the PLS coating prepared in Example 1 after being corroded by AgCl molten salt; Figure 5 The Ag element surface distribution of the Ag whiskers grown spontaneously in the cross section of the PLS coating prepared in Example 1 after being corroded by AgCl molten salt; Figure 6 The surface distribution of Ag element of the Ag whiskers grown spontaneously in the cross section of the sample of the PLS coating prepared in Example 1 after being corroded by AgCl molten salt and ground by sandpaper; Figure 7 This is a cross-sectional microstructure diagram of the PLS coating of Example 2 after being corroded by AgCl molten salt; Figure 8 Cr element distribution diagram of the cross section of the PLS coating prepared in Example 2 after being corroded by AgCl molten salt; Fig. 9 The Ag element distribution diagram of the cross section of the PLS coating prepared in Example 2 after being corroded by AgCl molten salt; Fig.10 Ag whiskers grown spontaneously in the cross section of the PLS coating prepared in Example 2 after being corroded by AgCl molten salt; Fig.11 This is a cross-sectional microstructure diagram of the PLS coating of Example 3 after being corroded by AgCl molten salt; Fig.12 This is the Ag element distribution diagram of the cross section of the PLS coating prepared in Example 3 after being corroded by AgCl molten salt. DETAILED DESCRIPTION

[0020] The technical solution of the present invention will be further described below in conjunction with the accompanying drawings.

[0021] It is clear and complete that the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In the following examples, the periodic lamellar structure (PLS) coating is prepared by the following method: Step 1: Cut the prepared Fe-(15-30)wt.%Cr-(4-7)wt.%B cast steel into samples of 70mm*10mm*4mm in size, suspend them with steel wire, and immerse them in Al-4.4wt.% Si melt for hot-dip aluminum reaction. The melt temperature is 750℃ and the hot-dip time is 30 minutes. Take it out after the time is reached and cool it to room temperature in air. Use wire cutting to cut the sample in the middle, prepare the metallographic sample after grinding and polishing, and observe its structure using the backscattered electron mode of a scanning electron microscope. It is found that PLS will be generated at the (Cr,Fe)2B / Al melt interface after hot-dip aluminum.

[0023] Step 2: Place the hot-dip aluminum sample in a muffle furnace for diffusion heat treatment at 750°C for 60 minutes, and cool it in the furnace. Cut the sample from the center using wire cutting, and observe the cross-sectional microstructure after grinding and polishing. It can be seen that the number and thickness of PLS ​​increase. The PLS coating can be prepared through the above two steps.

[0024] The PLS coating can be prepared through the above two steps.

[0025] Fe-Cr-B cast steel is prepared by the following steps: Step 1: Ingredients: According to the designed alloy composition, calculate the required weight of low-carbon ferrochromium Fe-58wt.%Cr-0.06wt.%C, Fe-18 wt.%B master alloy and pig iron, with a total weight of 10kg.

[0026] Step 2, smelting: the raw materials weighed in step 1 are placed in a vacuum melting furnace, and after being completely melted, they are superheated to 1600°C and kept warm for 15 minutes, and then poured into a metal mold, and after cooling, Fe-Cr-B cast steel is obtained.

[0027] The microstructure of the prepared Fe-Cr-B cast steel is mainly composed of gray-black (Cr,Fe)2B phase and gray-white α-Fe. The microstructure in the embodiment is photographed using a backscattered electron mode of a scanning electron microscope. The whiter the contrast, the larger the average atomic number.

[0028] Embodiment 1: The prepared Fe-Cr-B cast steel containing PLS coating was immersed in AgCl molten salt at 600℃ and taken out after 5 minutes to obtain a small amount of Ag-substituted PLS coating. After grinding and polishing, the cross-sectional microstructure was observed using the backscattered electron mode of a scanning electron microscope, such as Figure 1 As shown, it can be observed that the position of the original Cr-Al-B MAB phase in PLS is obviously "whitened", and the substitution of Ag can be easily observed.

[0029] Among them, the surface distribution of Cr and Ag elements are as follows: Figure 2 , 3 As shown in the figure, the Cr element represents the position of the original Cr-Al-BMAB phase in the PLS. It can be seen that the position of the Cr-Al-B MAB phase in the PLS coating after being corroded by the AgCl molten salt is obviously "white", and its Ag content is relatively high, indicating that the Cr-Al-B MAB phase in the PLS coating reacted chemically with the AgCl molten salt after being corroded by the AgCl molten salt, partially replacing the Al atoms in the Cr-Al-B MAB phase and generating a pure Ag phase. After the polished sample was placed for 7 days, irregularly shaped Ag whiskers spontaneously grew on the above-mentioned whitened Cr-Al-B MAB phase area, and their morphology and element surface distribution were shown as follows: Figure 4 , 5 shown.

[0030] The sample obtained after AgCl molten salt corrosion was prepared into a metallographic specimen after sandpaper grinding and polishing, and immediately placed in a scanning electron microscope. After 10 hours, prismatic Ag whiskers could be seen, such as Figure 6 shown.

[0031] Embodiment 2: The prepared Fe-Cr-B cast steel containing PLS coating was immersed in AgCl molten salt at a temperature of 750°C and taken out after 5 minutes to obtain a large amount of Ag-substituted PLS coating. After grinding and polishing, the cross-sectional microstructure was observed using the backscattered electron mode of a scanning electron microscope, such as Figure 7 As shown in Figure 2, it can be observed that the position of the original Cr-Al-B MAB phase in the PLS is obviously "white", and the corresponding surface distributions of the two elements Cr and Ag are as follows: Figure 8 , 9 As shown, compared with Example 1, Example 2 is more "white", and Ag is further enriched on the interface of Cr-Al-B MAB phase / FeAl3. At the same time, the pure Ag phase in the adjacent whitish Cr-Al-B MAB phase area in PLS grows relatively and penetrates the FeAl3 in the middle. This shows that with the increase of reaction temperature, the replacement efficiency of Ag is significantly improved, and pure Ag also grows along the FeAl3 grain boundary. After the polished sample was placed for 7 days, irregularly shaped Ag whiskers spontaneously grew in the above-mentioned whitish PLS coating area (including the Cr-Al-B MAB phase and FeAl3 areas), as shown in Figure 2. Fig.10 shown.

[0032] Embodiment 3: The prepared Fe-Cr-B cast steel containing PLS coating was immersed in AgCl molten salt at a temperature of 750°C and taken out after 30 minutes to obtain a large amount of Ag-substituted PLS coating. After grinding and polishing, the cross-sectional microstructure was observed using the backscattered electron mode of a scanning electron microscope, such as Fig.11 As shown in Figure 2, the surface distribution of Ag element is as follows: Fig.12 As shown in the figure, it is found that with the extension of reaction time, the whitening degree of Cr-Al-B MAB phase does not increase significantly, but the FeAl3 phase has been completely penetrated by Ag, and the remaining FeAl3 phase is scattered in the form of "islands" at the original position of the FeAl3 phase in PLS. This shows that after being corroded by 750℃ AgCl molten salt for 30 minutes, the Ag in the molten salt + The replacement reaction with the Cr-Al-B MAB phase in PLS has reached saturation. +It mainly reacts with the FeAl3 phase and generates a Fe-Al-Ag ternary compound, which makes the entire PLS area white. At the same time, due to the high Ag content in the FeAl3 phase area, the contrast of the Cr-Al-B MAB phase area decreases and becomes "black" in comparison. After the polished sample was placed for 3 days, Ag whiskers spontaneously grew in the above-mentioned whitened PLS coating area (including the Cr-Al-B MAB phase and the FeAl3 area).

[0033] The above embodiments are only preferred technical solutions of the invention and should not be regarded as limitations of the invention. The protection scope of the invention should be the technical solutions recorded in the claims, including equivalent replacement solutions of the technical features in the technical solutions recorded in the claims. That is, equivalent replacement improvements within this scope are also within the protection scope of the invention.

Claims

1. A material for spontaneously growing Ag whiskers, comprising a periodic lamellar structure coating, It is characterized in that The periodic lamellar structure coating includes a Cr-Al-B MAB phase containing Ag atoms.

2. A material for spontaneously growing Ag whiskers according to claim 1, It is characterized in that The Ag atoms exist in two forms, one is the Ag atoms in the Cr-Al-Ag-B MAB phase, and the other is the single substance Ag on the grain boundary of the Cr-Al-Ag-B MAB phase or the Cr-Al-BMAB phase.

3. A material for spontaneously growing Ag whiskers according to claim 1, It is characterized in that The Ag atoms in the periodic lamellar structure coating spontaneously generate Ag whiskers after being left to stand.

4. A material for spontaneously growing Ag whiskers according to claim 3, It is characterized in that The Ag whiskers are irregular or prismatic.

5. A method for preparing a material for spontaneously growing Ag whiskers according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Step 1: Preparation of periodic layer structure coating: The Fe-Cr-B cast steel was immersed in an Al-Si alloy melt for hot-dip plating. After hot-dip plating, the sample was quickly taken out of the alloy melt, air-cooled, and then subjected to diffusion heat treatment. The boride (Cr, Fe) in the Fe-Cr-B cast steel 2 The Cr-Al-B MAB phase and FeAl 3 A periodic lamellar structure coating composed of alternating layers; Step 2: AgCl molten salt corrosion: The specimen containing the periodic lamellar structure coating prepared in step 1 is immersed in AgCl molten salt for molten salt corrosion. The specimen taken out after the molten salt corrosion is cleaned by ultrasonic wave to remove the residual salt on the surface. The Cr-Al-B MAB phase in the periodic lamellar structure coating after the AgCl molten salt corrosion contains Ag atoms.

6. A method for preparing a material for spontaneously growing Ag whiskers according to claim 5, It is characterized in that In the step 2, the temperature of the AgCl molten salt is 600-800° C., and the test piece containing the periodic lamellar structure coating is immersed in the AgCl molten salt for corrosion for 5 minutes to 120 minutes.

7. A method for preparing a material for spontaneously growing Ag whiskers according to claim 5, It is characterized in that In the step 2, the Ag atoms in the periodic lamellar structure coating after AgCl molten salt corrosion come from Ag in the AgCl molten salt. + .

8. A method for preparing a material for spontaneously growing Ag whiskers according to claim 5, It is characterized in that In the step 2, the chemical reaction between the Cr-Al-B MAB phase and the AgCl molten salt in the periodic lamellar structure coating is: Cr-Al-BMAB phase + AgCl → Cr-Al-Ag-B MAB phase + AlCl 3 + Ag.

9. A method for preparing a material for spontaneously growing Ag whiskers according to claim 5, It is characterized in that In the step 2, the AgCl molten salt reacts chemically with the Cr-Al-B MAB phase in the periodic lamellar structure coating first; as the temperature of the AgCl molten salt increases and the corrosion time increases, the FeAl 3 It reacts with AgCl molten salt to form Fe-Al-Ag ternary phase.

10. A method for preparing a material for spontaneously growing Ag whiskers according to claim 5, It is characterized in that The single substance Ag in the periodic lamellar structure coating after AgCl molten salt corrosion is discontinuously distributed in the entire Cr-Al-B MAB phase region, and the self-grown Ag whiskers are also discontinuously distributed.