Preparation process of wear-resistant viscose cotton blended yarn

The wear resistance and deformation resistance of the adhesive cotton-blended yarn are solved by using the blend ratio of 50% cotton fiber and 50% viscose fiber in the adhesive cotton-blended yarn and adhering a modified polyaniline modification layer on the surface of the yarn. The problem of insufficient results has achieved higher wear resistance and deformation resistance, reduced the generation of pom pom, and improved the service life of clothes and the quality of clothing.

CN118880508APending Publication Date: 2024-11-01FUJIAN SPRUCE TEXTILE TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410911345.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing cotton-blended yarn has poor wear resistance and deformation resistance, and it is prone to problems of pompoon and pattern changes.

Method used

Using a blend ratio of 50% cotton fiber and 50% viscose fiber, and a modified polyaniline modification layer is attached to the surface of the yarn. Through a specific spinning process and surface modification process, a continuous polyaniline layer is formed to improve wear resistance. and deformation resistance.

Benefits of technology

It effectively reduces the pom pom from the yarn due to friction, improves the wear resistance and deformation resistance of the yarn, ensures that the shape of the clothes is not easy to change after long-term use, and has excellent anti-static effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004933682070000061
    Figure BDA0004933682070000061
  • Figure BDA0004933682070000071
    Figure BDA0004933682070000071
  • Figure BDA0004933682070000091
    Figure BDA0004933682070000091
Patent Text Reader

Abstract

The invention relates to the technical field of mixed spinning processes, in particular to a preparation process of wear-resistant viscose cotton blended yarn. The preparation technology of the wear-resistant viscose cotton blended yarn sequentially comprises the following steps of opening picking, cotton carding, drawing, roving, spinning, spooling and surface modification. The wear-resistant viscose cotton blended yarn comprises cotton fibers with the fiber content blending ratio being 50% and viscose fibers with the fiber content blending ratio being 50%, and a modified polyaniline modification layer is attached to the surface of the wear-resistant viscose cotton blended yarn. The wear-resistant viscose cotton blended yarn has excellent wear resistance, deformation resistance and antistatic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of mixed spinning technology, and more specifically, it relates to a preparation process of wear-resistant viscose-cotton blended yarn. Background Art

[0002] With the increasing development of social economy and the improvement of people's living standards, people's consumption concepts are constantly updated. They pay more and more attention to the quality of life and living environment, and have higher and higher functional requirements for clothing, especially the style and service life of clothing.

[0003] Viscose-cotton blended yarn is a composite yarn made of viscose fiber and cotton fiber. Viscose fiber refers to α-cellulose extracted from cellulose raw materials such as wood and plant stems, which is processed into spinning solution and then wet-spun to produce artificial fibers. Viscose-cotton blended yarn combines the characteristics of cotton and viscose fibers. Therefore, in addition to the comfort and breathability of cotton, it also has the softness and gloss of viscose fibers.

[0004] However, both cotton fiber and viscose fiber have poor wear resistance. After long-term use of clothes made of viscose-cotton blended yarn, fluff easily appears on the surface of the clothes due to friction. At the same time, the elastic modulus of cotton fiber and viscose fiber is low, so viscose-cotton blended yarn is easy to deform under a small load, and the elastic recovery performance is poor, which leads to the clothes made of viscose-cotton blended yarn being easy to change in shape after long-term use. Therefore, there is an urgent need for a viscose-cotton blended yarn with excellent wear resistance and deformation resistance. Summary of the invention

[0005] In order to improve the defects of poor wear resistance and deformation resistance of conventional viscose-cotton blended yarn, the present application provides a preparation process of wear-resistant viscose-cotton blended yarn.

[0006] The present application provides a preparation process for wear-resistant viscose-cotton blended yarn, which adopts the following technical solution: A preparation process of a wear-resistant viscose-cotton blended yarn, wherein the wear-resistant viscose-cotton blended yarn comprises a blending ratio of 50% cotton fiber and 50% viscose fiber, and a modified polyaniline modification layer is attached to the surface of the wear-resistant viscose-cotton blended yarn; The preparation process of the wear-resistant viscose-cotton blended yarn comprises the following steps: Cotton opening and cleaning process: Adopting the process principle of "more loosening and less beating, more recovery and less elimination, combing instead of beating", it is carried out through the cooperation of automatic cotton plucking machine, mixed cotton opening machine, cotton opening machine, cotton feeding machine and lap forming machine; The beater speed of the automatic plucking machine is 700-800r / min, the plucking trolley drops 2-4mm every time it runs, the blade extends 2-5mm from the rib, and the trolley runs at a speed of 1-3r / min; the double-row beater speed of the mixed cotton opener is 700-800r / min; the cotton opener speed is 500-600r / min, the lap machine speed is 600-800r / min, and the lap roller speed is 10-15r / min; After the cotton cleaning process, the viscose fiber roll length is 27m, the meter weight is 390g, and the meter weight unevenness rate is less than 1.0%; the cotton fiber roll length is 36m, the meter weight is 420g, and the meter weight unevenness rate is less than 1%; Carding process: adopt the process principle of "less grabbing, light beating, early falling and less falling", the cylinder speed is 400-450r / min, the licker-in speed is 1000-1100r / min, the flat speed is 80-100mm / min, and the distance between the cylinder and the flat from the inlet to the outlet is 0.18mm, 0.20mm, 0.13mm, and 0.13mm respectively; Drawing process: During production, the viscose fiber and the cotton fiber are pre-drawn and then mixed. The drafting multiples in the post-drawing zone are 1.4-1.7, and the drafting multiples in the post-mixing zone are 1.5-1.95. The pre-drawing is 3 viscose fibers and 3 cotton fibers. The front roller spacing is 10-14mm, the middle roller spacing is 2-8mm, the back roller spacing is 18-22mm, and the delivery speed is 260-280m / min. Roving process: adopting the process principle of "large gauge, large twist coefficient, small back draft", the back zone drafting multiple is 1.3-1.4, the front roller center distance is 5-10mm, the middle roller center distance is 20-26mm, the back roller center distance is 30-35mm, the spindle speed is 900-1000r / min, the twist coefficient is 98-108, the total mechanical drafting multiple is 9-10, and the basis weight is 3.0-4.0g / 10m; Spinning process: Siro spinning technology is adopted, double coarse sand is fed in the spinning drafting area, the yarn guide stroke is 6-8mm, a larger back zone interval and a larger back zone drafting multiple are adopted, the back zone drafting multiple is 1.38-1.50, the front roller center distance is 40-46mm, the back roller center distance is 70-76mm, the spindle speed is 14000-15000r / min, the spacing block is 2.0-2.5mm, the twist coefficient is 330-360, the front roller speed is 190-200r / min, and the total drafting speed is 45-55; Winding process: winding speed 1000-1350r / min, to obtain pre-treated viscose-cotton blended yarn; Surface modification process: modifying the pretreated viscose-cotton blended yarn, attaching a polyaniline modification layer on the surface of the pretreated viscose-cotton blended yarn, and obtaining the wear-resistant viscose-cotton blended yarn.

[0007] Preferably, the specific steps of the surface modification process are: immersing the pretreated viscose-cotton blended yarn in an acetone solution, removing impurities on the surface of the pretreated viscose-cotton blended yarn by ultrasonication for 20-40 minutes, and then vacuum drying; then adding the dried wear-resistant viscose-cotton blended yarn to a 30-50°C hydrochloric acid aqueous solution for 1-2 hours, and then adding the modified aniline composition, mixing and stirring at 30-50°C for 1-3 hours, and then adding an ammonium persulfate aqueous solution, mixing at 30-50°C, and then filtering, and washing with acetone and deionized water, and finally vacuum drying to obtain the wear-resistant viscose-cotton blended yarn.

[0008] When the above-mentioned surface modification process is adopted, the aniline monomer will form a larger hydrogen bond interaction with the surface of the pretreated viscose-cotton blended yarn, thereby loading a large amount of aniline monomer on the surface of the pretreated viscose-cotton blended yarn, and the aniline monomer will gradually grow into a continuous layer along the template of the pretreated viscose-cotton blended yarn, and then completely cover the pretreated viscose-cotton blended yarn, thereby eliminating the direct contact between the viscose-cotton blended yarn and the outside world, effectively reducing the possibility of fluff generated by friction on the viscose-cotton blended yarn, that is, effectively improving the wear resistance of the viscose-cotton blended yarn.

[0009] At the same time, since polyaniline has a high elastic modulus, its mechanical properties are extremely good. Therefore, when the surface of the pretreated viscose-cotton blended yarn is coated with a continuous layer of polyaniline, the prepared wear-resistant viscose-cotton blended yarn will also have a high elastic modulus. Therefore, after the clothes woven with the wear-resistant viscose-cotton blended yarn are used for a long time, their pattern is still not easy to change, that is, they obtain excellent anti-deformation performance.

[0010] In addition, the polyaniline continuous layer also has extremely good electrical conductivity, thereby enabling the prepared wear-resistant viscose-cotton blended yarn to have excellent antistatic effect.

[0011] Preferably, in the surface modification process, the amount of the dried pretreated viscose-cotton blended yarn added is 0.5 g, the concentration of the hydrochloric acid aqueous solution is 0.02-0.03 M / 100 ml, the amount of the hydrochloric acid aqueous solution added is 200 ml, the content of aniline monomer in the modified aniline composition is 0.04-0.06 M, the concentration of the ammonium persulfate aqueous solution is 0.07-0.09 M / 100 ml, and the amount of the ammonium persulfate aqueous solution added is 100 ml.

[0012] In the surface modification process, when the components are used in the above concentrations, the wear-resistant viscose-cotton blended yarn prepared will have better wear resistance and tensile strength.

[0013] Preferably, in the surface modification step, after adding the aqueous ammonium persulfate solution, the mixture is mixed at 30-50° C. for 4-12 hours.

[0014] After adding ammonium persulfate aqueous solution, the mechanical properties and wear resistance of the wear-resistant viscose-cotton blended yarn gradually improved with the increase of mixing time. However, when the mixing time exceeded 8h, the mechanical properties and wear resistance of the wear-resistant viscose-cotton blended yarn slightly decreased.

[0015] The reason may be that, in the early stage, the mechanical properties of the viscose-cotton blended yarn were reduced due to the corrosion of hydrochloric acid. As the mixing time increased, a polyaniline continuous layer was gradually formed on the surface of the viscose-cotton blended yarn, which led to a significant improvement in its mechanical properties and wear resistance. However, when the mixing time exceeded 8 hours, the polyaniline continuous layer no longer completely covered the viscose-cotton blended yarn, possibly due to irregular changes in the polyaniline continuous layer, which led to a decrease in the mechanical properties and wear resistance of the viscose-cotton blended yarn.

[0016] Preferably, graphene two-dimensional nanosheets are added to the modified aniline composition.

[0017] When graphene two-dimensional nanosheets are dispersed in a continuous layer of polyaniline, the graphene sheets with high modulus and large aspect ratio can effectively prevent and inhibit the migration of polymer chain segments, while transferring part of the external stress, thereby enabling the wear-resistant viscose-cotton blended yarn to obtain better anti-deformation properties.

[0018] In addition, since the carbon atoms in the graphene two-dimensional material are bonded by strong covalent bonds, it has very high strength and hardness, and the atomic arrangement structure on the graphene surface also causes it to have an extremely low friction coefficient. Therefore, when the graphene two-dimensional nanosheets are dispersed in the polyaniline continuous layer, the wear-resistant viscose-cotton blended yarn will obtain better wear resistance.

[0019] Preferably, the modified aniline composition is obtained by mixing aniline, graphene two-dimensional nanosheets, 4,4-diaminodiphenyl ether and trimellitic anhydride.

[0020] Preferably, the preparation method of the modified aniline composition is: first, aniline, graphene two-dimensional nanosheets and solvent methyl pyrrolidone are mixed by ultrasound for 1-2 hours, and then 4,4-diaminodiphenyl ether and trimellitic anhydride are added in sequence, and mixed and stirred for 12-36 hours under a nitrogen atmosphere at room temperature to obtain a modified aniline composition.

[0021] Preferably, in the modified aniline composition, the aniline content is 0.04-0.06M, the graphene two-dimensional nanosheets are 0.02-0.04g, the methyl pyrrolidone is 25-35ml, the 4,4-diaminodiphenyl ether is 1-3g, and the trimellitic anhydride is 1-3g.

[0022] Preferably, in the surface modification process, the parameters of vacuum drying are: temperature 200-400° C., and drying time 1-3 h.

[0023] When the modified aniline composition adopts the above components and addition amounts, at a temperature of 200-400°C and a drying time of 1-3h, methylpyrrolidone is first removed, and then other components are gradually imidized, so that while a polyaniline continuous layer system is obtained, a polyimide system is also formed, thereby enabling the wear-resistant viscose-cotton blended yarn to obtain better anti-sex performance and wear resistance.

[0024] In summary, this application has the following beneficial effects: 1. When the above-mentioned surface modification process is adopted, the aniline monomer will form a larger hydrogen bond interaction with the surface of the pretreated viscose-cotton blended yarn, thereby loading a large amount of aniline monomer on the surface of the pretreated viscose-cotton blended yarn, and the aniline monomer will gradually grow into a continuous layer along the template of the pretreated viscose-cotton blended yarn, and then completely cover the pretreated viscose-cotton blended yarn, thereby eliminating the direct contact between the viscose-cotton blended yarn and the outside world, effectively reducing the possibility of fluff generated by friction on the viscose-cotton blended yarn, that is, effectively improving the wear resistance of the viscose-cotton blended yarn.

[0025] 2. Since polyaniline has a high elastic modulus and excellent mechanical properties, when the surface of the pretreated viscose-cotton blended yarn is coated with a continuous layer of polyaniline, the prepared wear-resistant viscose-cotton blended yarn will also have a high elastic modulus. Therefore, after the clothes woven with the wear-resistant viscose-cotton blended yarn are used for a long time, their pattern is still not easy to change, that is, they have excellent anti-deformation performance.

[0026] 3. When graphene two-dimensional nanosheets are dispersed in the continuous layer of polyaniline, the graphene sheets with high modulus and large aspect ratio can effectively prevent and inhibit the migration of polymer segments, while transferring part of the external stress, thereby enabling the wear-resistant viscose-cotton blended yarn to obtain better anti-deformation performance; In addition, since the carbon atoms in the graphene two-dimensional material are bonded by strong covalent bonds, it has very high strength and hardness, and the atomic arrangement structure on the graphene surface also causes it to have an extremely low friction coefficient. Therefore, when the graphene two-dimensional nanosheets are dispersed in the polyaniline continuous layer, the wear-resistant viscose-cotton blended yarn will obtain better wear resistance. DETAILED DESCRIPTION

[0027] The present application is further described in detail below in conjunction with Examples 1-11 and Comparative Examples 1-2.

[0028] raw material Cotton fiber and viscose fiber are commercially available; acetone CAS: 67-64-1; hydrochloric acid CAS: 7647-01-0; ammonium persulfate CAS: 7727-54-0; aniline CAS: 62-53-3; graphene two-dimensional nanosheets Beike Nano; 4,4-diaminodiphenyl ether CAS: 101-80-4; trimellitic anhydride CAS: 552-30-7; methyl pyrrolidone CAS: 872-50-4. Example

[0029] Example 1 A preparation process of a wear-resistant viscose-cotton blended yarn, wherein the wear-resistant viscose-cotton blended yarn comprises cotton fibers with a blending ratio of 50% and viscose fibers with a blending ratio of 50%, and a modified polyaniline modification layer is attached to the surface of the wear-resistant viscose-cotton blended yarn; The preparation process of wear-resistant viscose-cotton blended yarn comprises the following steps: Cotton opening and cleaning process: Adopting the process principle of "more loosening and less beating, more recovery and less elimination, combing instead of beating", it is carried out through the cooperation of automatic cotton plucking machine, mixed cotton opening machine, cotton opening machine, cotton feeding machine and lap forming machine; The beater speed of the automatic plucking machine is 750r / min, the plucking trolley drops 3mm after each operation, the blade extends 3mm from the rib, and the trolley runs at a speed of 2r / min; the double-row beater speed of the mixed cotton opener is 750r / min; the cotton opener speed is 550r / min, the lap machine speed is 700r / min, and the lap roller speed is 13r / min; After the cotton cleaning process, the viscose fiber roll length is 27m, the meter weight is 390g, and the meter weight unevenness rate is less than 1.0%; the cotton fiber roll length is 36m, the meter weight is 420g, and the meter weight unevenness rate is less than 1%; Carding process: Adopt the process principle of "less grabbing, light beating, early falling and less falling", the cylinder speed is 420r / min, the licker-in speed is 1050r / min, the flat speed is 90mm / min, and the cylinder and flat gauges from inlet to outlet are 0.18mm, 0.20mm, 0.13mm, and 0.13mm respectively; Drawing process: During production, the viscose fiber and the cotton fiber are pre-drawn and then mixed. The drafting multiples in the post-drawing zone are 1.6, and the drafting multiples in the post-mixing zone are 1.7. The pre-drawing is 3 viscose fibers and 3 cotton fibers. The front roller spacing is 12mm, the middle roller spacing is 6mm, the back roller spacing is 20mm, and the delivery speed is 270m / min. Roving process: adopting the process principle of "large gauge, large twist coefficient, small back draft", the back zone drafting multiple is 1.4, the front roller center distance is 7mm, the middle roller center distance is 24mm, the back roller center distance is 32mm, the spindle speed is 950r / min, the twist coefficient is 102, the total mechanical drafting multiple is 10, and the basis weight is 3.5g / 10m; Spinning process: Siro spinning technology is adopted, double coarse sand is fed in the spinning drafting area, the yarn guide stroke is 8mm, a larger back zone interval and a larger back zone drafting multiple are adopted, the back zone drafting multiple is 1.50, the front roller center distance is 44mm, the back roller center distance is 73mm, the spindle speed is 14500r / min, the spacing block is 2.3mm, the twist coefficient is 340, the front roller speed is 200r / min, and the total drafting speed is 50; Winding process: winding speed 1200r / min, to obtain pre-treated viscose-cotton blended yarn; Surface modification process: soak the pretreated viscose-cotton blended yarn in an acetone solution, remove impurities on the surface of the pretreated viscose-cotton blended yarn by ultrasonic treatment for 30 minutes, and then vacuum dry it at a drying temperature of 100°C; then add the dried wear-resistant viscose-cotton blended yarn to a 40°C hydrochloric acid aqueous solution for 2 hours, then add aniline, mix and stir at 40°C for 2 hours, then add an ammonium persulfate aqueous solution, mix at 40°C, then filter, and wash with acetone and deionized water, and finally vacuum dry it at a drying temperature of 300°C for 2 hours to obtain the wear-resistant viscose-cotton blended yarn; Among them, the added amount of the dried wear-resistant viscose-cotton blended yarn is 0.5g, the concentration of the hydrochloric acid aqueous solution is 0.025M / 100ml, the added amount of the hydrochloric acid aqueous solution is 200ml, the added amount of aniline is 0.05M, the concentration of the ammonium persulfate aqueous solution is 0.08M / 100ml, and the added amount of the ammonium persulfate aqueous solution is 100ml.

[0030] Example 2-3 The difference from Example 1 is that, when the amount of added wear-resistant viscose-cotton blended yarn after drying is 0.5 g, the concentration of the hydrochloric acid aqueous solution, the amount of aniline added and the concentration of the ammonium persulfate aqueous solution are different, as shown in Table 1.

[0031] Table 1: Addition amount of each component in the surface modification process of Examples 1-3 Example 1 Example 2 Example 3 Concentration of hydrochloric acid aqueous solution (M / 100ml) 0.025 0.02 0.03 Aniline addition amount M 0.05 0.06 0.04 Ammonium persulfate aqueous solution concentration (M / 100ml) 0.08 0.07 0.09 Example 4 The difference from Example 1 is that in the surface modification step, after adding the aqueous ammonium persulfate solution, the mixture was mixed at 40° C. for 4 hours.

[0032] Example 5 The difference from Example 1 is that in the surface modification step, after adding the aqueous ammonium persulfate solution, the mixture was mixed at 40° C. for 12 hours.

[0033] Example 6 The difference from Example 1 is that 0.03 g of graphene two-dimensional nanosheets are further added to aniline.

[0034] Example 7 The difference from Example 1 is that aniline is replaced by a modified aniline composition; The preparation method of the modified aniline composition is as follows: firstly, aniline, graphene two-dimensional nanosheets and solvent methyl pyrrolidone are mixed by ultrasonication for 2 hours, then 4,4-diaminodiphenyl ether and trimellitic anhydride are added in sequence, and the mixture is mixed and stirred for 24 hours under a nitrogen atmosphere at room temperature to obtain the modified aniline composition; Among them, the aniline content is 0.05M, the graphene two-dimensional nanosheet is 0.03g, the methyl pyrrolidone is 30ml, the 4,4-diaminodiphenyl ether is 2.1g, and the trimellitic anhydride is 1.9g.

[0035] Embodiment 8-9 The difference from Example 7 is that the added amounts of the components of the modified aniline composition are different, as shown in Table 2.

[0036] Table 2 Addition amount of each component of the modified aniline composition in Examples 7-9 Example 10 The difference from Example 7 is that in the surface modification process, the parameters of vacuum drying after washing are: temperature 200° C., drying time 1 h.

[0037] Embodiment 11 The difference from Example 7 is that in the surface modification process, the parameters of vacuum drying after washing are: temperature 400° C., drying time 3 h.

[0038] Comparative Example Comparative Example 1 A preparation process of viscose-cotton blended yarn, wherein the wear-resistant viscose-cotton blended yarn comprises cotton fiber with a blending ratio of 50% and viscose fiber with a blending ratio of 50%; The preparation process of viscose-cotton blended yarn comprises the following steps: Cotton opening and cleaning process: Adopting the process principle of "more loosening and less beating, more recovery and less elimination, combing instead of beating", it is carried out through the cooperation of automatic cotton plucking machine, mixed cotton opening machine, cotton opening machine, cotton feeding machine and lap forming machine; The beater speed of the automatic plucking machine is 750r / min, the plucking trolley drops 3mm after each operation, the blade extends 3mm from the rib, and the trolley runs at a speed of 2r / min; the double-row beater speed of the mixed cotton opener is 750r / min; the cotton opener speed is 550r / min, the lap machine speed is 700r / min, and the lap roller speed is 13r / min; After the cotton cleaning process, the viscose fiber roll length is 27m, the meter weight is 390g, and the meter weight unevenness rate is less than 1.0%; the cotton fiber roll length is 36m, the meter weight is 420g, and the meter weight unevenness rate is less than 1%; Carding process: Adopt the process principle of "less grabbing, light beating, early falling and less falling", the cylinder speed is 420r / min, the licker-in speed is 1050r / min, the flat speed is 90mm / min, and the cylinder and flat gauges from inlet to outlet are 0.18mm, 0.20mm, 0.13mm, and 0.13mm respectively; Drawing process: During production, the viscose fiber and the cotton fiber are pre-drawn and then mixed. The drafting multiples in the post-drawing zone are 1.6, and the drafting multiples in the post-mixing zone are 1.7. The pre-drawing is 3 viscose fibers and 3 cotton fibers. The front roller spacing is 12mm, the middle roller spacing is 6mm, the back roller spacing is 20mm, and the delivery speed is 270m / min. Roving process: adopting the process principle of "large gauge, large twist coefficient, small back draft", the back zone drafting multiple is 1.4, the front roller center distance is 7mm, the middle roller center distance is 24mm, the back roller center distance is 32mm, the spindle speed is 950r / min, the twist coefficient is 102, the total mechanical drafting multiple is 10, and the basis weight is 3.5g / 10m; Spinning process: Siro spinning technology is adopted, double coarse sand is fed in the spinning drafting area, the yarn guide stroke is 8mm, a larger back zone interval and a larger back zone drafting multiple are adopted, the back zone drafting multiple is 1.50, the front roller center distance is 44mm, the back roller center distance is 73mm, the spindle speed is 14500r / min, the spacing block is 2.3mm, the twist coefficient is 340, the front roller speed is 200r / min, and the total drafting speed is 50; Winding process: winding speed 1200r / min, to obtain viscose-cotton blended yarn.

[0039] Comparative Example 2 A preparation process of a wear-resistant viscose-cotton blended yarn, wherein the wear-resistant viscose-cotton blended yarn comprises cotton fibers with a blending ratio of 50% and viscose fibers with a blending ratio of 50%, and a polyaniline layer is attached to the surface of the wear-resistant viscose-cotton blended yarn; The preparation process of viscose-cotton blended yarn comprises the following steps: Cotton opening and cleaning process: Adopting the process principle of "more loosening and less beating, more recovery and less elimination, combing instead of beating", it is carried out through the cooperation of automatic cotton plucking machine, mixed cotton opening machine, cotton opening machine, cotton feeding machine and lap forming machine; The beater speed of the automatic plucking machine is 750r / min, the plucking trolley drops 3mm after each operation, the blade extends 3mm from the rib, and the trolley runs at a speed of 2r / min; the double-row beater speed of the mixed cotton opener is 750r / min; the cotton opener speed is 550r / min, the lap machine speed is 700r / min, and the lap roller speed is 13r / min; After the cotton cleaning process, the viscose fiber roll length is 27m, the meter weight is 390g, and the meter weight unevenness rate is less than 1.0%; the cotton fiber roll length is 36m, the meter weight is 420g, and the meter weight unevenness rate is less than 1%; Carding process: Adopt the process principle of "less grabbing, light beating, early falling and less falling", the cylinder speed is 420r / min, the licker-in speed is 1050r / min, the flat speed is 90mm / min, and the cylinder and flat gauges from inlet to outlet are 0.18mm, 0.20mm, 0.13mm, and 0.13mm respectively; Drawing process: During production, the viscose fiber and the cotton fiber are pre-drawn and then mixed. The drafting multiples in the post-drawing zone are 1.6, and the drafting multiples in the post-mixing zone are 1.7. The pre-drawing is 3 viscose fibers and 3 cotton fibers. The front roller spacing is 12mm, the middle roller spacing is 6mm, the back roller spacing is 20mm, and the delivery speed is 270m / min. Roving process: adopting the process principle of "large gauge, large twist coefficient, small back draft", the back zone drafting multiple is 1.4, the front roller center distance is 7mm, the middle roller center distance is 24mm, the back roller center distance is 32mm, the spindle speed is 950r / min, the twist coefficient is 102, the total mechanical drafting multiple is 10, and the basis weight is 3.5g / 10m; Spinning process: Siro spinning technology is adopted, double coarse sand is fed in the spinning drafting area, the yarn guide stroke is 8mm, a larger back zone interval and a larger back zone drafting multiple are adopted, the back zone drafting multiple is 1.50, the front roller center distance is 44mm, the back roller center distance is 73mm, the spindle speed is 14500r / min, the spacing block is 2.3mm, the twist coefficient is 340, the front roller speed is 200r / min, and the total drafting speed is 50; Winding process: winding speed 1200r / min, to obtain pre-treated viscose-cotton blended yarn; Surface modification process: soak the pretreated viscose-cotton blended yarn in aniline for 2 hours, with the added amount of aniline being 0.05M based on the added amount of the dried pretreated viscose-cotton blended yarn being 0.5g, and then take it out and vacuum dry it at a drying temperature of 300°C for a drying time of 2 hours to obtain a wear-resistant viscose-cotton blended yarn.

[0040] Performance testing Detection Methods 1. Tensile performance test Three samples were taken from Examples 1-11 and Comparative Examples 1-2, respectively, and the tensile strength of the samples was tested according to GB / T 14344-2022 “Test Method for Tensile Properties of Chemical Fiber Filaments”, and the average value was taken.

[0041] 2. Wear resistance test Three samples were taken out from Examples 1-11 and Comparative Examples 1-2 respectively, and then the original mass of the samples was weighed, which was recorded as M0; thereafter, all the samples were put on a roller, and then the samples were controlled to be transported on the roller. The roller was made of stainless steel, and the surface of the roller was provided with anti-slip strips. After all the samples were transported, the surface conditions of the samples were observed and the actual mass was weighed, which was recorded as M1. Finally, the wear value was calculated to characterize the wear resistance of the samples; the wear value = M0-M1, and the average value was taken.

[0042] The test data are shown in Table 3.

[0043] Table 3 Test data table of Examples 1-11 and Comparative Examples 1-3 With reference to Examples 1-11 and Comparative Examples 1-2 and in combination with Table 3, it can be seen that a large number of fuzz balls appeared after the wear test in Comparative Example 1, a small amount of fuzz balls appeared after the wear test in Comparative Example 2, and the surface conditions of other Examples or Comparative Examples were normal. This shows that attaching a polyaniline connecting layer on the surface of the viscose-cotton blended yarn can effectively improve the wear resistance of the viscose-cotton blended yarn, thereby improving the generation of fuzz balls to a certain extent.

[0044] With reference to Example 1 and Comparative Examples 1-2 and in combination with Table 3, it can be seen that, relative to Comparative Example 1, the tensile strength of Comparative Example 2 is slightly improved, the wear resistance of Comparative Example 2 is significantly reduced, and the surface pilling condition of Comparative Example 2 is also greatly improved; at the same time, relative to Comparative Example 2, the tensile strength of Example 1 is further improved, the wear resistance of Example 1 is further significantly reduced, and the surface pilling condition of Example 1 becomes normal, which shows that, relative to the pure use of aniline, the surface modification process of Example 1 can enable the viscose-cotton blended yarn to obtain better tensile properties and wear resistance.

[0045] The reason is that when the above-mentioned surface modification process is adopted, the aniline monomer will form a larger hydrogen bond interaction with the surface of the pretreated viscose-cotton blended yarn, thereby loading a large amount of aniline monomer on the surface of the pretreated viscose-cotton blended yarn, and the aniline monomer will gradually grow into a continuous layer along the template of the pretreated viscose-cotton blended yarn, and then completely cover the pretreated viscose-cotton blended yarn, thereby eliminating the direct contact between the viscose-cotton blended yarn and the outside world, effectively reducing the possibility of fluff generated by friction on the viscose-cotton blended yarn, that is, effectively improving the wear resistance of the viscose-cotton blended yarn.

[0046] In addition, since polyaniline has a high elastic modulus and excellent mechanical properties, when the surface of the pretreated viscose-cotton blended yarn is coated with a continuous layer of polyaniline, the prepared wear-resistant viscose-cotton blended yarn will also have a high elastic modulus. Therefore, after the clothing woven with the wear-resistant viscose-cotton blended yarn is used for a long time, its pattern is still not easy to change, that is, it obtains excellent anti-deformation performance.

[0047] With reference to Examples 1-3 and in combination with Table 3, it can be seen that, relative to Example 1, the tensile strength of Examples 2-3 is slightly decreased, while the wear value of Example 2 is slightly increased. This indicates that when the components of the surface modification process are added in the amounts of Example 1, the wear-resistant viscose-cotton blended yarn prepared will have better tensile and wear resistance.

[0048] With reference to Example 1 and Examples 4-5 and in combination with Table 3, it can be seen that, relative to Example 1, the tensile strength of Examples 4-5 is significantly reduced, and the wear values ​​of Examples 4-5 are significantly improved. This shows that after adding the ammonium persulfate aqueous solution, the mixing time of the mixing thermometer of Example 1 can make the wear-resistant viscose-cotton blended yarn have better wear resistance and tensile properties.

[0049] The reason is that, in the early stage, the mechanical properties of the viscose-cotton blended yarn were reduced due to the corrosion of hydrochloric acid. As the mixing time increased, a polyaniline continuous layer was gradually formed on the surface of the viscose-cotton blended yarn, which led to a significant improvement in its mechanical properties and wear resistance. However, when the mixing time exceeded 8 hours, the polyaniline continuous layer no longer completely covered the viscose-cotton blended yarn, possibly due to irregular changes in the polyaniline continuous layer, which led to a decrease in the mechanical properties and wear resistance of the viscose-cotton blended yarn.

[0050] Referring to Example 1 and Example 6 and combining with Table 3, it can be seen that, relative to Example 1, the tensile strength of Example 6 is significantly improved, and the wear value of Example 6 is significantly reduced, which shows that the addition of graphene two-dimensional nanosheets can effectively improve the wear resistance and tensile properties of the wear-resistant viscose-cotton blended yarn.

[0051] The reason is that when graphene two-dimensional nanosheets are dispersed in the continuous layer of polyaniline, the graphene sheets with high modulus and large aspect ratio can effectively prevent and inhibit the migration of polymer segments, while transferring part of the external stress, thereby enabling the wear-resistant viscose-cotton blended yarn to obtain better anti-deformation performance; In addition, since the carbon atoms in the graphene two-dimensional material are bonded by strong covalent bonds, it has very high strength and hardness, and the atomic arrangement structure on the graphene surface also causes it to have an extremely low friction coefficient. Therefore, when the graphene two-dimensional nanosheets are dispersed in the polyaniline continuous layer, the wear-resistant viscose-cotton blended yarn will obtain better wear resistance.

[0052] Referring to Examples 6-7 and in combination with Table 3, it can be seen that, relative to Example 6, the tensile strength of Example 7 is further improved, and the abrasion value of Example 7 is further reduced, which indicates that the provision of the modified aniline composition can further improve the wear resistance and tensile properties of the wear-resistant viscose-cotton blended yarn.

[0053] The reason is that when the modified aniline composition adopts the above-mentioned components and addition amounts, at a temperature of 300°C and a drying time of 2h, methylpyrrolidone is removed first, and then the other components are gradually imidized, so that while obtaining a polyaniline continuous layer system, a polyimide system is also formed, thereby enabling the wear-resistant viscose-cotton blended yarn to obtain better anti-gender performance and wear resistance.

[0054] With reference to Examples 7-11 and in combination with Table 3, it can be seen that, relative to Example 7, the tensile strength of Examples 8-11 is reduced to varying degrees, and the wear values ​​of Examples 8-11 are increased to varying degrees. This indicates that when the components and processes of the surface modification process use the addition amounts and parameters of Example 7, the wear-resistant viscose-cotton blended yarn prepared will have better wear resistance and tensile properties.

[0055] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A process for preparing wear-resistant viscose-cotton blended yarn, characterized in that: The wear-resistant viscose-cotton blended yarn comprises a blending ratio of 50% cotton fiber and 50% viscose fiber, and a modified polyaniline modification layer is attached to the surface of the wear-resistant viscose-cotton blended yarn; The preparation process of the wear-resistant viscose-cotton blended yarn comprises the following steps: Cotton opening and cleaning process: Adopting the process principle of "more loosening and less beating, more recovery and less elimination, combing instead of beating", it is carried out through the cooperation of automatic cotton plucking machine, mixed cotton opening machine, cotton opening machine, cotton feeding machine and lap forming machine; The beater speed of the automatic plucking machine is 700-800r / min, the plucking trolley drops 2-4mm every time it runs, the blade extends 2-5mm from the rib, and the trolley runs at a speed of 1-3r / min; the double-row beater speed of the mixed cotton opener is 700-800r / min; the cotton opener speed is 500-600r / min, the lap machine speed is 600-800r / min, and the lap roller speed is 10-15r / min; After the cotton cleaning process, the viscose fiber roll length is 27m, the meter weight is 390g, and the meter weight unevenness rate is less than 1.0%; the cotton fiber roll length is 36m, the meter weight is 420g, and the meter weight unevenness rate is less than 1%; Carding process: Adopt the process principle of "less grabbing, light beating, early dropping and less dropping", the cylinder speed is 400-450r / min, the licker-in speed is 1000-1100r / min, the flat speed is 80-100mm / min, and the distance between the cylinder and the flat from the inlet to the outlet is 0.18mm, 0.20mm, 0.13mm, and 0.13mm respectively; Drawing process: During production, the viscose fiber and the cotton fiber are pre-drawn and then mixed. The drafting multiples in the post-drawing zone are 1.4-1.7, and the drafting multiples in the post-mixing zone are 1.5-1.

95. The pre-drawing is 3 viscose fibers and 3 cotton fibers. The front roller spacing is 10-14mm, the middle roller spacing is 2-8mm, the back roller spacing is 18-22mm, and the delivery speed is 260-280m / min. Roving process: adopt the process principle of "large gauge, large twist coefficient, small back draft", the back zone draft multiple is 1.3-1.4, the front roller center distance is 5-10mm, the middle roller center distance is 20-26mm, the back roller center distance is 30-35mm, the spindle speed is 900-1000r / min, the twist coefficient is 98-108, the total mechanical draft multiple is 9-10, and the basis weight is 3.0-4.0g / 10m; Spinning process: Siro spinning technology is adopted, double coarse sand is fed in the spinning drafting area, the yarn guide stroke is 6-8mm, a larger back zone interval and a larger back zone drafting multiple are adopted, the back zone drafting multiple is 1.38-1.50, the front roller center distance is 40-46mm, the back roller center distance is 70-76mm, the spindle speed is 14000-15000r / min, the spacing block is 2.0-2.5mm, the twist coefficient is 330-360, the front roller speed is 190-200r / min, and the total drafting speed is 45-55; Winding process: winding speed 1000-1350r / min, to obtain pre-treated viscose-cotton blended yarn; Surface modification process: modifying the pretreated viscose-cotton blended yarn, attaching a polyaniline modification layer on the surface of the pretreated viscose-cotton blended yarn, and obtaining the wear-resistant viscose-cotton blended yarn.

2. The preparation process of the wear-resistant viscose-cotton blended yarn according to claim 1, characterized in that: The specific steps of the surface modification process are: immersing the pretreated viscose-cotton blended yarn in an acetone solution, removing impurities on the surface of the pretreated viscose-cotton blended yarn by ultrasonic treatment for 20-40 minutes, and then vacuum drying; then adding the dried wear-resistant viscose-cotton blended yarn to a 30-50°C hydrochloric acid aqueous solution for 1-2 hours, and then adding the modified aniline composition, mixing and stirring at 30-50°C for 1-3 hours, and then adding an ammonium persulfate aqueous solution, mixing at 30-50°C, and then filtering, and washing with acetone and deionized water, and finally vacuum drying to obtain the wear-resistant viscose-cotton blended yarn.

3. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 2, characterized in that: In the surface modification process, the amount of the dried pretreated viscose-cotton blended yarn added is 0.5 g, the concentration of the hydrochloric acid aqueous solution is 0.02-0.03 M / 100 ml, the amount of the hydrochloric acid aqueous solution added is 200 ml, the content of aniline monomer in the modified aniline composition is 0.04-0.06 M, the concentration of the ammonium persulfate aqueous solution is 0.07-0.09 M / 100 ml, and the amount of the ammonium persulfate aqueous solution added is 100 ml.

4. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 3, characterized in that: In the surface modification process, after adding the ammonium persulfate aqueous solution, the mixture is mixed at 30-50° C. for 4-12 hours.

5. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 2, characterized in that: The modified aniline composition is added with graphene two-dimensional nanosheets.

6. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 5, characterized in that: The modified aniline composition is obtained by mixing aniline, graphene two-dimensional nanosheets, 4,4-diaminodiphenyl ether and trimellitic anhydride.

7. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 6, characterized in that: The preparation method of the modified aniline composition is as follows: firstly, aniline, graphene two-dimensional nanosheets and solvent methyl pyrrolidone are mixed by ultrasonic treatment for 1-2 hours, then 4,4-diaminodiphenyl ether and trimellitic anhydride are added in sequence, and the mixture is mixed and stirred for 12-36 hours under a nitrogen atmosphere at room temperature to obtain the modified aniline composition.

8. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 7, characterized in that: The modified aniline composition contains 0.04-0.06M aniline, 0.02-0.04g of graphene two-dimensional nanosheets, 25-35ml of methyl pyrrolidone, 1-3g of 4,4-diaminodiphenyl ether and 1-3g of trimellitic anhydride.

9. The process for preparing the wear-resistant viscose-cotton blended yarn according to claim 8, characterized in that: In the surface modification process, the parameters of vacuum drying after washing are: temperature 200-400° C., and drying time 1-3 hours.

Citation Information

Patent Citations

  • Cotton fiber and viscose blended yarn and manufacturing method thereof

    CN103088496A

  • Method for preparing animal hair composite fiber by virtue of functional polymer modification and composite hair fiber and fabric prepared by virtue of method

    CN106758255A

  • Graphene reinforced polyimide nanometer composite material, preparation method and applications thereof

    CN108203543A

  • Blending spinning technology for combing polyester and viscose

    CN108611718A

  • Wear-resistant and scratch-resistant modification method of leather for bags and suitcases

    CN111138937A