Graphene oxide-based PN junction and preparation method and application thereof

The graphene oxide-based PN junction is constructed through the π-bond conjugation effect between aromatic hydrocarbons and graphene oxide sheets, which solves the problems of high-temperature energy consumption and structural unevenness in the preparation process of inorganic semiconductor PN junction materials, and realizes graphene oxide-based PN junction The uniformity and photoelectric responsiveness of PN junctions are suitable for flexible surfaces and large-scale production.

CN118890950APending Publication Date: 2024-11-01CHINA UNIV OF MINING & TECH (BEIJING)
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410966660.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the preparation process, existing inorganic semiconductor PN junction materials have problems such as high temperature energy consumption, uncontrollable bandwidth, uneven structure and active chemical properties, making them difficult to be suitable for flexible surfaces or large-scale production.

Method used

Using the π bond conjugation effect between aromatic hydrocarbons and graphene oxide sheet layers, an N-type and P-type graphene oxide layer was formed on the conductive substrate through ultrasonic atomization spraying process to construct graphene oxide-based PN junction, avoiding chemical reactions and B/N atomic substitution process to achieve precise control of bandwidth and structural uniformity of bandwidth.

Benefits of technology

The graphene oxide-based PN junction has good structural uniformity, uniform texture, significant rectification characteristics and photoelectric response capabilities. It is suitable for large-size preparation and large-scale production, avoiding the use of flammable and explosive materials, and improving safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890950A_ABST
    Figure CN118890950A_ABST
Patent Text Reader

Abstract

The invention provides a graphene oxide-based PN junction and a preparation method and application thereof, and relates to the technical field of semiconductor elements. The graphene oxide-based PN junction comprises a conductive substrate, an N-type graphene oxide layer, a P-type graphene oxide layer and a silver electrode which are stacked in sequence. Wherein the N-type graphene oxide layer comprises an aromatic hydrocarbon compound with electron donating performance and graphene oxide; wherein the P-type graphene oxide layer comprises an aromatic hydrocarbon compound with electron withdrawing performance and graphene oxide. The graphene oxide-based PN junction is good in structural uniformity and uniform in texture, and has remarkable rectification characteristics and photoelectric response capability; meanwhile, the influence of a B / N atom substitution chemical reaction process on the forbidden bandwidth of the graphene oxide can be avoided, and the forbidden bandwidth of the graphene oxide-based PN junction can be accurately controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor components, and in particular to a graphene oxide-based PN junction and a preparation method and application thereof. Background Art

[0002] PN junction is an extremely important semiconductor structure, generally formed by close contact between P-type semiconductor and N-type semiconductor. Due to the difference in carrier concentration between the two semiconductors in the PN junction, the holes with a higher concentration in the P-type semiconductor (P region) will spontaneously drift to the N-type semiconductor, and the electrons with a higher concentration in the N-type semiconductor (N region) will also spontaneously drift to the P-type semiconductor. Since the drift of holes and electrons leaves fixed donor ions and acceptor ions without carrier compensation in the P region and N region respectively, an electric field is formed at the interface between the P region and the N region, which points from the N-type semiconductor to the P-type semiconductor, that is, the built-in electric field. The region where the built-in electric field is located is called the space charge region. An important characteristic of the PN junction is its unidirectional conductivity: when the P region is connected to the positive pole of the external power supply and the N region is connected to the negative pole of the external power supply, the external electric field can offset the built-in electric field, and the carriers can move under the action of the external electric field to form a continuous forward current; when the P region is connected to the negative pole of the external power supply and the N region is connected to the positive pole of the external power supply, the external electric field increases the resistance of the built-in electric field, the PN junction cannot be turned on, and there is only a very weak reverse current. Another important characteristic of the PN junction is its photoelectric effect. When a forward voltage is applied to the PN junction, under the action of the external electric field, the holes in the P-type semiconductor and the electrons in the N-type semiconductor recombine in the space charge region and release energy in the form of photons. When the PN junction is irradiated with light of an appropriate wavelength, electrons and holes are generated in the space charge region by photon excitation, and move to the N region and the P region respectively under the action of the built-in electric field to form a photo-generated electromotive force. Due to its unique unidirectional conductivity and photoelectric effect, the PN junction is widely used as a core component in semiconductor devices such as logic gates, light-emitting diodes and photovoltaic cells.

[0003] Traditional PN junctions are mainly constructed by using inorganic semiconductor materials such as silicon, gallium arsenide, and germanium through element doping. With the rapid development of the semiconductor industry, inorganic semiconductor PN junctions have gradually shown the following shortcomings: (1) The band gap width of inorganic semiconductor PN junctions lacks plasticity; (2) The preparation and doping process of inorganic semiconductor PN junctions must be carried out at high temperatures, which consumes a lot of energy; (3) The reserves of inorganic semiconductor materials such as arsenic, gallium, indium, and germanium are limited, which makes it difficult to meet the growing demand for semiconductors; (4) Inorganic semiconductor materials are generally rigid and brittle, making them difficult to apply to flexible surfaces or curved substrates.

[0004] Based on the above situation, researchers proposed to use graphene oxide materials to construct PN junctions. Graphene oxide materials are derivatives of graphene materials and are generally prepared by aqueous phase graphite oxidation. The preparation process of graphene oxide materials is mild, with low energy consumption, and its band structure is adjustable, suitable for flexible surfaces, and is expected to become a new generation of PN junction materials. Graphene oxide-based PN junctions are mainly composed of P-type graphene oxide layers and N-type graphene oxide layers. Generally, a layer of N-type graphene oxide layer is first prepared on the surface of the substrate, and then a layer of P-type graphene oxide layer is prepared on top of the N-type graphene oxide layer. The preparation method of the currently widely used P-type / N-type graphene oxide layer is similar to that of P-type / N-type inorganic semiconductors. By replacing some C atoms in graphene oxide with B or N, holes or free electrons are introduced to make graphene oxide have the properties of P-type semiconductors or N-type semiconductors. The commonly used process route is to use NaBH4 or N2H4 to react with graphene oxide, and realize the substitution of B or N for C atoms on the graphene oxide sheet during the reaction. However, the preparation method of the P-type / N-type graphene oxide layer has the following main deficiencies: (1) The reaction of NaBH4 / N2H4 with graphene oxide is a reduction reaction, which has a great influence on the band gap width of graphene oxide, and is not conducive to the control of the band structure and band gap width of graphene oxide-based PN junction; (2) The reaction process of NaBH4 / N2H4 with graphene oxide is relatively intense, which has a negative impact on the structural uniformity of graphene oxide-based PN junction, and is not conducive to the preparation of large-size graphene oxide-based PN junction; (3) NaBH4 / N2H4 is flammable and has active chemical properties. It is flammable and explosive in the air and is not suitable for large-scale graphene oxide-based PN junction production.

[0005] Therefore, how to rationally construct graphene oxide-based PN junctions and optimize the preparation process of graphene oxide-based PN junctions has become a key research target in PN junction material science and engineering.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The purpose of the present invention is to provide a graphene oxide-based PN junction and its preparation method and application. The graphene oxide-based PN junction comprises a conductive substrate, an N-type graphene oxide layer, a P-type graphene oxide layer and a silver electrode stacked in sequence; wherein the N-type graphene oxide layer comprises an aromatic hydrocarbon compound with electron-donating properties and graphene oxide; wherein the P-type graphene oxide layer comprises an aromatic hydrocarbon compound with electron-withdrawing properties and graphene oxide. The graphene oxide-based PN junction of the present invention has good structural uniformity, uniform texture, and has significant rectification characteristics and photoelectric response capabilities.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] In a first aspect, the present invention provides a graphene oxide-based PN junction, wherein the graphene oxide-based PN junction comprises a conductive substrate, an N-type graphene oxide layer, a P-type graphene oxide layer, and a silver electrode stacked in sequence;

[0010] Wherein, the N-type graphene oxide layer comprises an aromatic hydrocarbon compound having electron-donating properties and graphene oxide;

[0011] Wherein, the P-type graphene oxide layer includes an aromatic hydrocarbon compound with electron-withdrawing properties and graphene oxide.

[0012] In the present invention, the N-type graphene oxide layer, the P-type graphene oxide layer and the silver electrode (i.e., the P-region electrode) are sequentially formed on the surface of the conductive substrate (i.e., the N-region electrode); wherein the N-type graphene oxide layer contains an aromatic hydrocarbon compound with electron-donating properties, and the P-type graphene oxide layer includes an aromatic hydrocarbon compound with electron-withdrawing properties, and the graphene oxide-based PN junction in the vertical direction is constructed by close contact between the N-type graphene oxide layer and the P-type graphene oxide layer. Moreover, the graphene oxide-based PN junction of the present invention can make the graphene oxide sheet have P-type or N-type semiconductor properties without chemical reaction by means of the π bond conjugation effect between the aromatic hydrocarbon and the graphene oxide sheet; at the same time, the influence of the B / N atomic substitution chemical reaction process on the graphene oxide band gap width can be avoided, and the accurate control of the graphene oxide-based PN junction band gap width can be achieved. Moreover, the graphene oxide-based PN junction of the present invention has good structural uniformity, uniform texture, and has significant rectification characteristics and photoelectric response capabilities.

[0013] Preferably, the length of the conductive substrate is 10 to 1000 mm, for example, it can be 10 mm, 20 mm, 40 mm, 60 mm, 80 mm, 100 mm, 150 mm, 200 mm, 250 mm, 300 mm, 350 mm, 400 mm, 500 mm, 600 mm, 700 mm, 800 mm, 900 mm, 1000 mm, etc.

[0014] Preferably, the width of the conductive substrate is 10 to 1000 mm, for example, it can be 10 mm, 20 mm, 40 mm, 60 mm, 80 mm, 100 mm, 150 mm, 200 mm, 250 mm, 300 mm, 350 mm, 400 mm, 500 mm, 600 mm, 700 mm, 800 mm, 900 mm, 1000 mm, etc.

[0015] Preferably, the thickness of the conductive substrate is less than 5 mm, for example, it may be 5 mm, 4.5 mm, 4 mm, 3.5 mm, 3 mm, 2.5 mm, 2 mm, 1.5 mm, 1 mm, etc.

[0016] In the present invention, the substrate is generally a sheet structure, and the length, width and thickness can be determined by actual needs. It should be noted that the scheme described in the present invention does not involve chemical reactions, the process is mild, and is suitable for large-scale liquid phase film forming technology and large-scale PN junction preparation needs.

[0017] Preferably, the surface roughness of the conductive substrate is <50nm, for example, it can be 49nm, 45nm, 40nm, 35nm, 30nm, 25nm, 20nm, 15nm, 10nm, 9nm, 8.5nm, 8nm, 7.5nm, 7nm, 6.5nm, 6nm, 5.5nm, 5nm, 4.5nm, 4nm, 3.5nm, 3nm, 2.5nm, 2nm, 1.5nm, 1nm, etc., preferably <10nm.

[0018] Preferably, the surface square resistance of the conductive substrate is <10Ω, for example, it may be 9Ω, 8Ω, 7Ω, 6Ω, 5Ω, 4.5Ω, 4Ω, 3.5Ω, 3Ω, 2.5Ω, 2Ω, 1.5Ω, 1Ω, 0.5Ω, etc., preferably <5Ω.

[0019] In the present invention, the base material should be an inorganic material with a flat and smooth surface (surface roughness should be <50nm, preferably <10nm) and good conductivity (surface square resistance <10Ω, preferably <5Ω).

[0020] Preferably, the material of the conductive substrate is selected from any one of copper, silver or ITO quartz or a combination of at least two thereof.

[0021] It should be noted that when the graphene oxide-based PN junction described in the present invention is used to prepare semiconductors such as diodes and logic gates that do not involve the photoelectric effect, copper, silver and other chemically stable and conductive metals or alloys can be used as substrate materials; and when the graphene oxide-based PN junction described in the present invention is used to prepare photovoltaic cells and other semiconductor applications involving the photoelectric effect, a transparent conductive material such as ITO quartz (quartz coated with an indium tin oxide layer) is preferably selected as the substrate material.

[0022] Preferably, the thickness of the N-type graphene oxide layer is 20 to 2000 nm, for example, it can be 20 nm, 40 nm, 60 nm, 80 nm, 90 nm, 100 nm, 120 nm, 140 nm, 160 nm, 180 nm, 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, 400 nm, 600 nm, 800 nm, 1000 nm, 1200 nm, 1400 nm, 1600 nm, 1800 nm, 2000 nm, etc., preferably 100 to 300 nm, and more preferably 200 nm.

[0023] Preferably, the mass ratio of the aromatic hydrocarbon compound having electron donating properties to graphene oxide is (0.05-0.5):1, for example, it can be 0.05:1, 0.06:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, 0.25:1, 0.28:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, preferably (0.1-0.3):1, and more preferably 0.2:1.

[0024] Preferably, the aromatic hydrocarbon compound having electron donating property is selected from amino and / or imino substituted aromatic hydrocarbon compounds; wherein the aromatic hydrocarbon compound is selected from any one or a combination of at least two of naphthalene, anthracene, phenanthrene or pyrene.

[0025] Preferably, the aromatic hydrocarbon compound having electron donating properties is selected from any one of 1-naphthylamine, 1,5-naphthalenediamine, 2-anthraceneamine, 5-anthraceneamine, N-phenyl-9-anthraceneamine, 2-phenanthramine, 9-phenanthramine, 1-pyreneamine, 4-pyreneamine, 1,6-pyrenediamine or 2,7-pyrenediamine, or a combination of at least two thereof.

[0026] Preferably, the thickness of the P-type graphene oxide layer is 200 to 5000 nm, for example, it can be 200 nm, 220 nm, 240 nm, 260 nm, 280 nm, 300 nm, 400 nm, 600 nm, 800 nm, 900 nm, 950 nm, 1000 nm, 1150 nm, 1200 nm, 1400 nm, 1600 nm, 1800 nm, 2000 nm, etc., preferably 800 to 1200 nm, and more preferably 1000 nm.

[0027] Preferably, the mass ratio of the electron-withdrawing aromatic compound to graphene oxide is (0.05-0.5):1, for example, it can be 0.05:1, 0.06:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, 0.25:1, 0.28:1, 0.3:1, 0.35:1, 0.4:1, 0.45:1, 0.5:1, preferably (0.1-0.3):1, and more preferably 0.2:1.

[0028] Preferably, the electron-withdrawing aromatic hydrocarbon compound is selected from nitro and / or sulfonyl substituted aromatic hydrocarbon compounds; wherein the aromatic hydrocarbon compound is selected from any one or a combination of at least two of naphthalene, anthracene, phenanthrene or pyrene.

[0029] Preferably, the electron-withdrawing aromatic hydrocarbon compound is selected from any one of 1-nitronaphthalene, 1-naphthalenesulfonic acid, 1,5-naphthalenedisulfonic acid, 3-nitrophenanthrene, 9-nitrophenanthrene, 9-phenanthrenesulfonic acid, 9-nitroanthracene, 2-nitroanthracene, 2-anthracenesulfonic acid, 1-pyrenesulfonic acid, 1-nitropyrene, 1,8-dinitropyrene or 1,3,6-trinitropyrene, or a combination of at least two thereof.

[0030] Preferably, the thickness of the silver electrode is greater than 10 μm, for example, it can be 10 μm, 20 μm, 40 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, etc.

[0031] In a second aspect, the present invention provides a method for preparing a graphene oxide-based PN junction as described in the first aspect, wherein the method for preparing a graphene oxide-based PN junction comprises the following steps:

[0032] An aromatic hydrocarbon compound with electron-donating properties, graphene oxide and an organic solvent are mixed to obtain a precursor solution of N-type graphene oxide; and an aromatic hydrocarbon compound with electron-withdrawing properties, graphene oxide and an organic solvent are mixed to obtain a precursor solution of P-type graphene oxide;

[0033] The conductive substrate is heated to a first temperature, and the precursor solution of the N-type graphene oxide is sprayed on the surface of the conductive substrate to form an N-type graphene oxide layer;

[0034] Heating the conductive substrate having the N-type graphene oxide layer to a second temperature, spraying the P-type graphene oxide precursor solution on the surface of the N-type graphene oxide layer to form a P-type graphene oxide layer;

[0035] A silver electrode is prepared on the surface of the P-type graphene oxide layer to obtain the graphene oxide-based PN junction.

[0036] In the present invention, the preparation method uses P-type / N-type aromatic hydrocarbons to modify graphene oxide, and through the π bond conjugation effect, the graphene oxide has P-type or N-type semiconductor properties, and through the liquid phase film forming technology, an N-type graphene oxide layer and a P-type graphene oxide layer are sequentially generated on the surface of a conductive smooth substrate, thereby realizing the preparation of a graphene oxide-based PN junction. Compared with the existing graphene oxide-based PN junction preparation process, the method of the present invention is easy to operate, the preparation process is mild, does not involve chemical reactions, can effectively ensure the structural integrity of the graphene oxide layer, is suitable for the preparation of large-size PN junctions, and does not involve the use of inflammable and explosive dangerous goods. The preparation process is safe and reliable, and is suitable for mass production of graphene oxide-based PN junctions.

[0037] The first temperature is 120-300°C, for example, 120°C, 140°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, etc., and the second temperature is ≤ the first temperature.

[0038] In the present invention, the conductive substrate needs to be heated to a first temperature (T1 = 120-300°C) for two main purposes: (1) within this temperature range, the organic solvent in the N-type graphene oxide precursor solution can be rapidly evaporated during ultrasonic atomization spraying, so that the solute therein forms an N-type graphene oxide layer; and (2) within this temperature range, the band gap width of the N-type graphene oxide can be regulated by thermal reduction.

[0039] In the present invention, the conductive substrate having an N-type graphene oxide layer needs to be heated to a second temperature (T2) for two main purposes: (1) to rapidly evaporate the organic solvent in the P-type graphene oxide precursor solution so that the solute therein rapidly forms a P-type graphene oxide layer; and (2) to regulate the bandgap width of the P-type graphene oxide by partial thermal reduction.

[0040] In addition, it should be noted that in order to avoid secondary reduction of the existing N-type graphene oxide during the reduction of P-type graphene oxide, which would affect its band structure, T2 should be ≤ T1.

[0041] Preferably, in the precursor solution of the N-type graphene oxide, the content of the graphene oxide is 0.05-0.5wt‰, for example, it can be 0.05wt‰, 0.06wt‰, 0.08wt‰, 0.1wt‰, 0.12wt‰, 0.15wt‰, 0.18wt‰, 0.2wt‰, 0.22wt‰, 0.25wt‰, 0.3wt‰, 0.35wt‰, 0.4wt‰, 0.45wt‰, 0.5wt‰, etc., preferably 0.1-0.3wt‰, and more preferably 0.2wt‰.

[0042] Preferably, in the precursor solution of the P-type graphene oxide, the content of the graphene oxide is 0.05-0.5wt‰, for example, it can be 0.05wt‰, 0.06wt‰, 0.08wt‰, 0.1wt‰, 0.12wt‰, 0.15wt‰, 0.18wt‰, 0.2wt‰, 0.22wt‰, 0.25wt‰, 0.3wt‰, 0.35wt‰, 0.4wt‰, 0.45wt‰, 0.5wt‰, etc., preferably 0.1-0.3wt‰, and more preferably 0.2wt‰.

[0043] In the present invention, the mass concentration of graphene oxide in the N-type / P-type graphene oxide precursor solution can be further adjusted by distillation / volatilization / addition of organic solvents, so that its mass concentration finally falls within the range of 0.05 to 0.5‰, preferably 0.2‰.

[0044] Preferably, the organic solvent is selected from any one of methanol, ethanol, propanol, isopropanol or acetone, or a combination of at least two thereof.

[0045] In the present invention, the organic solvent in the precursor solution of N-type graphene oxide and the precursor solution of P-type graphene oxide should be infinitely miscible with water, have a vaporization point not higher than 120°C, and can dissolve aromatic hydrocarbons, for example, C1-C5 straight-chain or branched alcohols and / or C2-C5 straight-chain or branched ketones, and suitable options include methanol, ethanol, propanol, isopropanol, acetone, etc.

[0046] Furthermore, the precursor solution of the N-type graphene oxide is prepared by the following steps:

[0047] Mixing an aromatic hydrocarbon compound having electron-donating properties with an organic solvent to obtain an N-type aromatic hydrocarbon organic solution;

[0048] mixing an aqueous solution of graphene oxide and an organic solvent to obtain a graphene oxide organic solution;

[0049] The N-type aromatic hydrocarbon organic solution and the graphene oxide organic solution are mixed to obtain the N-type graphene oxide precursor solution.

[0050] Preferably, in the N-type aromatic hydrocarbon organic solution, the mass percentage of the aromatic hydrocarbon compound with electron donating property is 2-10%, for example, it can be 2%, 2.5%, 3%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 6%, 6.5%, 7%, 8%, 9%, 10%, etc., preferably 4-6%, and more preferably 5%.

[0051] Furthermore, the precursor solution of the P-type graphene oxide is prepared by the following steps:

[0052] Mixing an aromatic hydrocarbon compound having electron-withdrawing properties with an organic solvent to obtain a P-type aromatic hydrocarbon organic solution;

[0053] mixing an aqueous solution of graphene oxide and an organic solvent to obtain a graphene oxide organic solution;

[0054] The P-type aromatic hydrocarbon organic solution and the graphene oxide organic solution are mixed to obtain the P-type graphene oxide precursor solution.

[0055] Preferably, in the P-type aromatic hydrocarbon organic solution, the mass percentage of the aromatic hydrocarbon compound with electron-withdrawing properties is 2 to 10%, for example, it can be 2%, 2.5%, 3%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 6%, 6.5%, 7%, 8%, 9%, 10%, etc., preferably 4 to 6%, and more preferably 5%.

[0056] Preferably, the aqueous solution of graphene oxide is prepared by oxidizing high-purity graphite (such as using hydrogen peroxide oxidation) and ultrasonically exfoliating high-purity graphite flakes; wherein the carbon element accounts for 45-47%, the hydrogen element accounts for <2%, the nitrogen element accounts for <2%, the sulfur element accounts for <1%, and the remaining elements are oxygen.

[0057] Preferably, in the graphene oxide organic solution, the mass percentage of the organic solvent is greater than 90%, for example, it may be 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, etc.

[0058] In the present invention, an N-type graphene oxide layer is prepared on the surface of a substrate, the substrate is placed on a hot stage, heated and the substrate surface reaches a specified temperature T1. The N-type graphene oxide precursor solution is evenly sprayed on the substrate surface using the ultrasonic atomization spraying process parameters described below, thereby preparing an N-type graphene oxide layer with a smooth surface, uniform texture and no structural defects.

[0059] Furthermore, in the process of preparing the N-type graphene oxide layer, the spraying adopts ultrasonic atomization spraying, and the specific parameter settings include:

[0060] The nozzle reciprocates in a zigzag motion.

[0061] The frequency range of the ultrasonic oscillation of the nozzle is 20000-100000 Hz, for example, it can be 20000 Hz, 30000 Hz, 40000 Hz, 50000 Hz, 60000 Hz, 70000 Hz, 80000 Hz, 90000 Hz, 100000 Hz, etc., preferably 50000-70000 Hz, more preferably 60000 Hz.

[0062] The infusion rate range of the liquid pump is 0.05-0.5 mL / min, for example, it can be 0.05 mL / min, 0.06 mL / min, 0.08 mL / min, 0.1 mL / min, 0.15 mL / min, 0.2 mL / min, 0.25 mL / min, 0.3 mL / min, 0.35 mL / min, 0.4 mL / min, 0.45 mL / min, 0.5 mL / min, etc., preferably 0.1-0.3 mL / min, and more preferably 0.2 mL / min.

[0063] The moving speed range of the nozzle is 2000~10000mm / min, for example, it can be 2000mm / min, 3000mm / min, 4000mm / min, 5000mm / min, 6000mm / min, 7000mm / min, 8000mm / min, 9000mm / min, 10000mm / min, etc., preferably 5000~7000mm / min, and more preferably 6000mm / min.

[0064] The spraying thickness of a single layer is 10 to 50 nm, for example, it can be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, etc., and the thickness of the N-type graphene oxide layer is made to a specified thickness by multi-layer stacking (the specified thickness is specifically: 20 to 2000 nm, preferably 100 to 300 nm, and more preferably 200 nm).

[0065] In the present invention, a P-type graphene oxide layer is prepared on top of an N-type graphene oxide layer. A substrate covered with an N-type graphene oxide layer is placed on a hot stage, heated, and the surface temperature of the N-type graphene oxide layer reaches a specified temperature T2. The P-type graphene oxide precursor solution is uniformly sprayed on top of the N-type graphene oxide layer using the ultrasonic atomization spraying process parameters described below to prepare a P-type graphene oxide layer with a smooth surface, uniform texture, and no structural defects.

[0066] Furthermore, in the process of preparing the P-type graphene oxide layer, the spraying adopts ultrasonic atomization spraying, and the specific parameter settings include:

[0067] The nozzle reciprocates in a zigzag motion.

[0068] The frequency range of the ultrasonic oscillation of the nozzle is 20000-100000 Hz, for example, it can be 20000 Hz, 30000 Hz, 40000 Hz, 50000 Hz, 60000 Hz, 70000 Hz, 80000 Hz, 90000 Hz, 100000 Hz, etc., preferably 50000-70000 Hz, more preferably 60000 Hz.

[0069] The infusion rate range of the liquid pump is 0.05-0.5 mL / min, for example, it can be 0.05 mL / min, 0.06 mL / min, 0.08 mL / min, 0.1 mL / min, 0.15 mL / min, 0.2 mL / min, 0.25 mL / min, 0.3 mL / min, 0.35 mL / min, 0.4 mL / min, 0.45 mL / min, 0.5 mL / min, etc., preferably 0.1-0.3 mL / min, and more preferably 0.2 mL / min.

[0070] The moving speed range of the nozzle is 2000~10000mm / min, for example, it can be 2000mm / min, 3000mm / min, 4000mm / min, 5000mm / min, 6000mm / min, 7000mm / min, 8000mm / min, 9000mm / min, 10000mm / min, etc., preferably 5000~7000mm / min, and more preferably 6000mm / min.

[0071] The single-layer spraying thickness is 10 to 50 nm, for example, it can be 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, etc.; the P-type graphene oxide layer is made to a specified thickness by multi-layer stacking (the specified thickness is specifically: 200 to 5000 nm, preferably 800 to 1200 nm, and more preferably 1000 nm).

[0072] Furthermore, the silver electrode is prepared by printing silver paste through inkjet printing technology.

[0073] In the present invention, the sample is cooled to room temperature, and silver paste is printed on the P-type graphene oxide layer using inkjet printing technology to form a silver electrode layer with a thickness of not less than 10 μm as the P-region electrode, thereby completing the preparation of the graphene oxide-based PN junction.

[0074] Preferably, the silver paste comprises, by mass percentage, 78-82% silver powder, 8-12% epoxy resin, 1-3% anhydride curing agent, 4-6% butyl acetate, and the remainder is active diluent.

[0075] Taking the total mass of the silver paste as 100%, the content of the silver powder is 78-82%, for example, 78%, 79%, 80%, 81%, 82%, etc.

[0076] Taking the total mass of the silver paste as 100%, the content of the epoxy resin is 8-12%, for example, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, etc.

[0077] Taking the total mass of the silver paste as 100%, the content of the anhydride curing agent is 1-3%, for example, it can be 1%, 1.2%, 1.4%, 1.6%, 1.8%, 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, etc.

[0078] Taking the total mass of the silver paste as 100%, the content of butyl acetate is 4-6%, for example, 4%, 4.2%, 4.4%, 4.6%, 4.8%, 5%, 5.2%, 5.4%, 5.6%, 5.8%, 6%, etc.

[0079] And / or, the epoxy resin is selected from bisphenol A epoxy resin, and the number average molecular weight of the bisphenol A epoxy resin is 3000-7000, for example, it can be 3000, 3500, 4000, 4500, 5000, 5500, 6000, 6500, 7000, etc.

[0080] And / or, the anhydride curing agent is selected from any one of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride or methyltetrahydrophthalic anhydride, or a combination of at least two thereof.

[0081] And / or, the reactive diluent is selected from any one or a combination of at least two of acrylate, propenyl glycidyl ether, phenyl glycidyl ether or resorcinol bisglycidyl ether.

[0082] In a third aspect, the present invention provides an application of the graphene oxide-based PN junction as described in the first aspect in the preparation of a semiconductor element.

[0083] In the present invention, the graphene oxide-based PN junction can be used to prepare semiconductor elements such as diodes, logic gates, and photovoltaic cells.

[0084] Compared with the prior art, the present invention has the following beneficial effects:

[0085] (1) The graphene oxide-based PN junction of the present invention can make the graphene oxide sheet have P-type or N-type semiconductor properties without chemical reaction by virtue of the π bond conjugation effect between aromatic hydrocarbons and graphene oxide sheets. The graphene oxide-based PN junction in the vertical direction is constructed by close contact between the N-type graphene oxide layer and the P-type graphene oxide layer. The PN junction has good structural uniformity, uniform texture, and has significant rectification characteristics and photoelectric response capabilities.

[0086] (2) Compared with the widely used method of preparing P-type / N-type graphene oxide layers by B / N atomic substitution, the preparation method of the present invention uses aromatic hydrocarbon adsorption to prepare the P-type / N-type graphene oxide layers, which avoids the influence of the B / N atomic substitution chemical reaction process on the band gap width of graphene oxide, and can achieve precise control of the band gap width of the graphene oxide-based PN junction.

[0087] (3) The adsorption modification of aromatic hydrocarbons in the preparation process of the present invention does not involve chemical reactions, and the process is mild, which is suitable for large-scale liquid phase film forming technology and large-scale PN junction preparation requirements; and the present invention avoids the use of chemically active, flammable and explosive NaBH4, N2H4, etc., which effectively improves the safety of large-scale production processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0088] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0089] Figure 1 Schematic diagram of the structure of the graphene oxide-based PN junction.

[0090] Among them, 101 is a conductive substrate, 102 is an N-type graphene oxide layer, 103 is a P-type graphene oxide layer, and 104 is a silver electrode.

[0091] Figure 2 The present invention is a process flow chart of the method for preparing the graphene oxide-based PN junction.

[0092] Figure 3 This is a microscopic morphology of the graphene oxide-based PN junction surface provided in Example 1.

[0093] Figure 4 This is a cross-sectional microscopic morphology of the graphene oxide-based PN junction provided in Example 21.

[0094] Figure 5 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 to 6.

[0095] Figure 6 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 and 7 to 10.

[0096] Figure 7 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 and 11 to 13.

[0097] Figure 8 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 and 14 to 17.

[0098] Fig. 9 This is a graph showing the test results of the ultraviolet-visible absorption spectrum of the N-type graphene oxide layer of the graphene oxide-based PN junction provided in Examples 1 to 6.

[0099] Fig.10 This is a graph showing the test results of the ultraviolet-visible absorption spectrum of the P-type graphene oxide layer of the graphene oxide-based PN junction provided in Examples 1 to 6. DETAILED DESCRIPTION

[0100] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.

[0101] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0102] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0103] Figure 1 is a schematic diagram of the structure of the graphene oxide-based PN junction, such as Figure 1 As shown, the graphene oxide-based PN junction includes a conductive substrate 101, an N-type graphene oxide layer 102, a P-type graphene oxide layer 103 and a silver electrode 104 stacked in sequence.

[0104] Figure 2 is a process flow chart of the method for preparing the graphene oxide-based PN junction of the present invention, as shown in Figure 2As shown, the preparation method comprises the following steps: mixing an aromatic hydrocarbon compound with electron-donating properties, graphene oxide and an organic solvent to obtain a precursor solution of N-type graphene oxide; at the same time, mixing an aromatic hydrocarbon compound with electron-withdrawing properties, graphene oxide and an organic solvent to obtain a precursor solution of P-type graphene oxide; heating the conductive substrate to a first temperature, spraying the precursor solution of N-type graphene oxide on the surface of the conductive substrate to form an N-type graphene oxide layer; heating the conductive substrate having the N-type graphene oxide layer to a second temperature, spraying the precursor solution of P-type graphene oxide on the surface of the N-type graphene oxide layer to form a P-type graphene oxide layer; preparing a silver electrode on the surface of the P-type graphene oxide layer to obtain the graphene oxide-based PN junction.

[0105] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.

[0106] Example 1

[0107] This embodiment provides a graphene oxide-based PN junction, which includes a conductive substrate, an N-type graphene oxide layer, a P-type graphene oxide layer, and a silver electrode stacked in sequence.

[0108] The substrate is a pure copper sheet of 20 mm × 30 mm × 1 mm; the surface roughness of the copper sheet is 100 nm, and the surface square resistance is 0.06 mΩ. The thickness of the N-type graphene oxide layer is 200 nm; the N-type graphene oxide layer includes 1,5-naphthalene diamine and graphene oxide in a mass ratio of 0.2:1. The thickness of the P-type graphene oxide layer is 1000 nm; the P-type graphene oxide layer includes 1,3,6-trinitropyrene and graphene oxide in a mass ratio of 0.2:1. The thickness of the silver electrode is 100 μm.

[0109] The graphene oxide-based PN junction described in this embodiment is prepared by the following steps:

[0110] S1. Preparation of precursor solution:

[0111] 1,5-naphthalenediamine and anhydrous ethanol are mixed to prepare a 1.0wt% 1,5-naphthalenediamine ethanol solution; 1,3,6-trinitropyrene and anhydrous ethanol are mixed to prepare a 1.0wt% 1,3,6-trinitropyrene ethanol solution; an aqueous solution of graphene oxide is diluted with anhydrous ethanol to prepare a 0.2wt‰ graphene oxide ethanol aqueous solution;

[0112] An ethanol solution of 1,5-naphthalene diamine and an ethanol aqueous solution of graphene oxide are mixed to prepare a precursor solution of N-type graphene oxide; wherein the mass ratio of 1,5-naphthalene diamine to graphene oxide is 0.2:1; an ethanol solution of 1,3,6-trinitropyrene and an ethanol aqueous solution of graphene oxide are mixed to prepare a precursor solution of P-type graphene oxide; wherein the mass ratio of 1,3,6-trinitropyrene to graphene oxide is 0.2:1.

[0113] S2. Preparation of N-type graphene oxide layer:

[0114] The substrate of the pure copper sheet is heated to 180° C., and the precursor solution of the N-type graphene oxide is sprayed on one side surface of the conductive substrate to form a 200 nm thick N-type graphene oxide layer. The N-type graphene oxide layer is completely dried at 180° C. for 1 hour, and the band gap width of the N-type graphene oxide reaches a specified energy value;

[0115] Among them, the spraying adopts ultrasonic atomization spraying, and the specific parameter settings include: the nozzle reciprocates in a zigzag shape; the frequency range of the ultrasonic oscillation of the nozzle is 60000Hz; the infusion rate range of the liquid pump is 0.2mL / min; the movement rate range of the nozzle is 6000mm / min; the spraying thickness of a single layer is 20nm; and the thickness of the N-type graphene oxide layer is made to a specified thickness of 200nm by multi-layer superposition.

[0116] S3. Preparation of P-type graphene oxide layer:

[0117] The conductive substrate having the N-type graphene oxide layer is heated to 180° C., and the precursor solution of the P-type graphene oxide is sprayed on one side surface of the conductive substrate to form a 1000 nm thick P-type graphene oxide layer. The P-type graphene oxide layer is completely dried at 180° C. for 1 hour, and the band gap width of the P-type graphene oxide reaches a specified energy value;

[0118] Among them, the spraying adopts ultrasonic atomization spraying, and the specific parameter settings include: the nozzle reciprocates in a zigzag shape; the frequency range of the ultrasonic oscillation of the nozzle is 60000Hz; the infusion rate range of the liquid pump is 0.2mL / min; the movement rate range of the nozzle is 6000mm / min; the spraying thickness of a single layer is 20nm; and the thickness of the N-type graphene oxide layer is made to a specified thickness of 1000nm by multi-layer superposition.

[0119] S4. Preparation of silver electrode:

[0120] The sample was cooled to room temperature, and silver paste was printed on the P-type graphene oxide layer using inkjet printing technology to form a 100 μm thick silver electrode layer;

[0121] The silver paste comprises, by mass percentage, 80% silver powder, 10% epoxy resin, 2% anhydride curing agent, 5% butyl acetate and 3% reactive diluent; the epoxy resin is bisphenol A epoxy resin, and the average number average molecular weight of the bisphenol A epoxy resin is 4500; the anhydride curing agent is phthalic anhydride; and the reactive diluent is acrylate.

[0122] Figure 3 The graphene oxide-based PN junction surface microscopic morphology provided in Example 1. Figure 3 As shown, the surface of the graphene oxide-based PN junction prepared in this embodiment is flat and has no structural defects, and has good consistency, which is conducive to forming a PN junction with stable performance.

[0123] Example 2

[0124] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is lowered to 140° C.; the temperature of the S3 conductive substrate having an N-type graphene oxide layer is lowered to 140° C.; other settings are exactly the same as Embodiment 1.

[0125] Example 3

[0126] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is reduced to 160° C.; the temperature of the S3 conductive substrate having an N-type graphene oxide layer is reduced to 160° C.; other settings are exactly the same as Embodiment 1.

[0127] Example 4

[0128] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is increased to 200° C.; the temperature of the S3 conductive substrate having an N-type graphene oxide layer is increased to 200° C.; other settings are completely consistent with Embodiment 1.

[0129] Example 5

[0130] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is increased to 225° C.; the temperature of the S3 conductive substrate having an N-type graphene oxide layer is increased to 225° C.; other settings are completely consistent with Embodiment 1.

[0131] Example 6

[0132] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is increased to 260°C; the temperature of the S3 conductive substrate having an N-type graphene oxide layer is increased to 260°C; the other settings are completely consistent with Embodiment 1.

[0133] Example 7

[0134] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of heating the conductive substrate S3 having an N-type graphene oxide layer is reduced to 140° C.; other settings are completely consistent with Embodiment 1.

[0135] Example 8

[0136] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of heating the conductive substrate S3 having an N-type graphene oxide layer is reduced to 160° C.; other settings are completely consistent with Embodiment 1.

[0137] Example 9

[0138] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is increased to 200° C.; other settings are completely consistent with Embodiment 1.

[0139] Example 10

[0140] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the temperature of the S2 conductive substrate is increased to 225° C.; other settings are completely consistent with Embodiment 1.

[0141] Embodiment 11

[0142] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that 1,5-naphthalene diamine is replaced by an equal mass of 1,6-pyrene diamine; 1,3,6-trinitropyrene is replaced by an equal mass of 1,6-dinitropyrene; and other settings are exactly the same as Embodiment 1.

[0143] Example 12

[0144] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that 1,5-naphthalenediamine is replaced by an equal mass of 1-anthraceneamine; 1,3,6-trinitropyrene is replaced by an equal mass of 1-nitroanthracene; and other settings are exactly the same as Embodiment 1.

[0145] Embodiment 13

[0146] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that 1,5-naphthalenediamine is replaced by an equal mass of 2-naphthylamine; 1,3,6-trinitropyrene is replaced by an equal mass of 2-nitronaphthalene; and other settings are exactly the same as Embodiment 1.

[0147] Embodiment 14

[0148] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the mass ratio of the 1,5-naphthalenediamine to the graphene oxide is changed to 0.05:1, and the mass ratio of the 1,3,6-trinitropyrene to the graphene oxide is changed to 0.05:1; other settings are completely consistent with Embodiment 1.

[0149] Embodiment 15

[0150] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the mass ratio of the 1,5-naphthalenediamine to the graphene oxide is changed to 0.1:1, and the mass ratio of the 1,3,6-trinitropyrene to the graphene oxide is changed to 0.1:1; other settings are completely consistent with Embodiment 1.

[0151] Example 16

[0152] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that the mass ratio of the 1,5-naphthalenediamine to the graphene oxide is changed to 0.35:1, and the mass ratio of the 1,3,6-trinitropyrene to the graphene oxide is changed to 0.35:1; other settings are completely consistent with Embodiment 1.

[0153] Embodiment 17

[0154] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the mass ratio of the 11,5-naphthalenediamine to the graphene oxide is changed to 0.5:1, and the mass ratio of the 11,3,6-trinitropyrene to the graphene oxide is changed to 0.5:1; other settings are completely consistent with Embodiment 1.

[0155] Embodiment 18

[0156] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the thickness of the P-type graphene oxide layer is reduced to 500 nm; other settings are completely consistent with Embodiment 1.

[0157] Embodiment 19

[0158] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the thickness of the P-type graphene oxide layer is increased to 2000 nm; other settings are completely consistent with Embodiment 1.

[0159] Embodiment 20

[0160] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the thickness of the N-type graphene oxide layer is reduced to 100 nm; other settings are completely consistent with Embodiment 1.

[0161] Embodiment 21

[0162] This embodiment provides a graphene oxide-based PN junction, which is different from Embodiment 1 only in that the thickness of the N-type graphene oxide layer is increased to 500 nm; other settings are completely consistent with Embodiment 1.

[0163] Figure 4 This is a cross-sectional microscopic morphology of a graphene oxide-based PN junction provided in Example 21. Figure 4 As shown, the N-type graphene oxide layer and the P-type graphene oxide layer of the graphene oxide-based PN junction prepared in this embodiment have a flat structure and good consistency, and the N-type graphene oxide layer and the P-type graphene oxide layer are tightly combined with a clear boundary, which is conducive to forming a PN junction with stable performance.

[0164] Embodiment 22

[0165] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that the pure copper sheet is replaced with an ITO quartz sheet of the same specification; other settings are exactly the same as Embodiment 1.

[0166] Comparative Example 1

[0167] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that 1,5-naphthalenediamine is replaced by 1,4-dimethylnaphthalene of equal mass; 1,3,6-trinitropyrene is replaced by 1,3,6-trimethylpyrene; and other settings are exactly the same as Embodiment 1.

[0168] Comparative Example 2

[0169] This embodiment provides a graphene oxide-based PN junction, which differs from Embodiment 1 only in that 1,5-naphthalenediamine is replaced by an equal mass of 2-chloronaphthalene; 1,3,6-trinitropyrene is replaced by 1-chloropyrene; and other settings are exactly the same as Embodiment 1.

[0170] Test Example 1

[0171] Test sample: graphene oxide-based PN junction provided in Examples 1 to 22;

[0172] Test method: Apply a DC voltage of -2.0V to +2.0V on both sides of the graphene oxide-based PN junction, and measure the current value passing through the graphene oxide-based PN junction; when the external voltage is forward biased, the voltage and current are recorded as positive values; when the external voltage is reverse biased, the voltage and current are recorded as negative values; record the current value every 0.1V; connect all data points to form a DC voltage-current curve test result diagram of the graphene oxide-based PN junction;

[0173] in, Figure 5 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 to 6. Figure 6 The DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 and 7 to 10 are shown. Figure 7 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 and 11 to 13. Figure 8 This is a graph showing the DC voltage-current curve test results of the graphene oxide-based PN junction provided in Examples 1 and 14 to 17.

[0174] like Figures 5 to 8 As shown, when a forward bias voltage and a reverse bias voltage with the same voltage value are applied, the current value of the graphene oxide-based PN junction under the forward bias voltage is significantly higher than the current value under the reverse bias voltage, and has significant PN junction rectification performance.

[0175] Test Example 2

[0176] Test sample: graphene oxide-based PN junction provided in Examples 1 to 6;

[0177] Test method: Place N-type and P-type graphene oxide films in a UV-visible absorption spectrometer to measure their UV-visible light absorption rates in the 200-800nm ​​band, and draw a UV-visible absorption spectrum test result graph based on their relative absorption rates;

[0178] in, Fig. 9 This is a graph showing the test results of the ultraviolet-visible absorption spectrum of the N-type graphene oxide layer of the graphene oxide-based PN junction provided in Examples 1 to 6. Fig.10 This is a graph showing the test results of the ultraviolet-visible absorption spectrum of the P-type graphene oxide layer of the graphene oxide-based PN junction provided in Examples 1 to 6.

[0179] like Figures 9-10 As shown in the figure, with the increase of heating temperature, the ultraviolet-visible light absorption peaks of the N-type graphene oxide layer and the P-type graphene oxide layer both show continuous red shift, which indicates that their light excitation band gap width gradually decreases with the increase of heating temperature. By controlling the heating temperature, the band gap width of the N-type graphene oxide layer and the P-type graphene oxide layer can be precisely controlled.

[0180] Test Example 3

[0181] Test samples: graphene oxide-based PN junctions provided in Examples 1 to 22, and graphene oxide-based PN junctions provided in Comparative Examples 1 to 2;

[0182] Test method:

[0183] The light-excited semiconductor bandgap of graphene oxide film is calculated by Tauc formula based on the UV-visible spectrum characterization results:

[0184] αhv=B(hv-E g ) n .

[0185] Where hν is the photon energy, α is the light absorption rate, E g is the bandgap width of the material's photoexcitation.

[0186] The rectification ratio of the graphene oxide-based PN junction of the present invention is obtained by calculating the ratio of the forward bias current to the reverse bias current at the same voltage.

[0187] The specific test results are shown in Table 1 below:

[0188] Table 1

[0189]

[0190]

[0191] As shown in Table 1, the rectification ratio of the graphene oxide-based PN junction of the present invention is 2.68-6.30, and a relatively high rectification ratio is obtained. The bandgap width of the N-type graphene oxide layer is 0.86-2.44 eV, and the bandgap width of the P-type graphene oxide layer is 0.96-2.68. When T1 or T2 does not change, the bandgap width of the N-type or P-type graphene oxide layer does not change by more than 0.05 eV, indicating that the graphene oxide-based PN junction of the present invention avoids the influence of the B / N atomic substitution chemical reaction process on the bandgap width of graphene oxide, and through thermal reduction, the bandgap width of the N-type / P-type graphene oxide reaches a specified energy value, so as to achieve precise control of the bandgap width of the graphene oxide-based PN junction.

[0192] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A graphene oxide-based PN junction, characterized in that: The graphene oxide-based PN junction comprises a conductive substrate, an N-type graphene oxide layer, a P-type graphene oxide layer and a silver electrode stacked in sequence; Wherein, the N-type graphene oxide layer comprises an aromatic hydrocarbon compound having electron-donating properties and graphene oxide; Wherein, the P-type graphene oxide layer includes an aromatic hydrocarbon compound with electron-withdrawing properties and graphene oxide.

2. The graphene oxide-based PN junction according to claim 1, characterized in that: The conductive substrate has a length of 10 to 1000 mm, a width of 10 to 1000 mm, and a thickness of less than 5 mm; And / or, the surface roughness of the conductive substrate is less than 50 nm; And / or, the surface square resistance of the conductive substrate is less than 10Ω; And / or, the material of the conductive substrate is selected from any one of copper, silver or ITO quartz or a combination of at least two thereof.

3. The graphene oxide-based PN junction according to claim 1, characterized in that: The thickness of the N-type graphene oxide layer is 20 to 2000 nm; And / or, the mass ratio of the aromatic hydrocarbon compound having electron donating property to graphene oxide is (0.05-0.5):1; And / or, the aromatic hydrocarbon compound having electron-donating properties is selected from amino and / or imino-substituted aromatic hydrocarbon compounds; wherein the aromatic hydrocarbon compound is selected from any one or a combination of at least two of naphthalene, anthracene, phenanthrene or pyrene; And / or, the aromatic hydrocarbon compound having electron donating properties is selected from any one of 1-naphthylamine, 1,5-naphthalenediamine, 2-anthraceneamine, 5-anthraceneamine, N-phenyl-9-anthraceneamine, 2-phenanthramine, 9-phenanthramine, 1-pyreneamine, 4-pyreneamine, 1,6-pyrenediamine or 2,7-pyrenediamine, or a combination of at least two thereof.

4. The graphene oxide-based PN junction according to claim 1, characterized in that: The thickness of the P-type graphene oxide layer is 200 to 5000 nm; And / or, the mass ratio of the electron-withdrawing aromatic hydrocarbon compound to graphene oxide is (0.05-0.5):1; And / or, the electron-withdrawing aromatic hydrocarbon compound is selected from nitro and / or sulfonyl substituted aromatic hydrocarbon compounds; wherein the aromatic hydrocarbon compound is selected from any one or a combination of at least two of naphthalene, anthracene, phenanthrene or pyrene; And / or, the aromatic hydrocarbon compound with electron-withdrawing properties is selected from any one or a combination of at least two of 1-nitronaphthalene, 1-naphthalenesulfonic acid, 1,5-naphthalenedisulfonic acid, 3-nitrophenanthrene, 9-nitrophenanthrene, 9-phenanthrenesulfonic acid, 9-nitroanthracene, 2-nitroanthracene, 2-anthracenesulfonic acid, 1-pyrenesulfonic acid, 1-nitropyrene, 1,8-dinitropyrene or 1,3,6-trinitropyrene.

5. The graphene oxide-based PN junction according to claim 1, characterized in that: The thickness of the silver electrode is greater than 10 μm.

6. A method for preparing a graphene oxide-based PN junction according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: An aromatic hydrocarbon compound with electron-donating properties, graphene oxide and an organic solvent are mixed to obtain a precursor solution of N-type graphene oxide; and an aromatic hydrocarbon compound with electron-withdrawing properties, graphene oxide and an organic solvent are mixed to obtain a precursor solution of P-type graphene oxide; The conductive substrate is heated to a first temperature, and the precursor solution of the N-type graphene oxide is sprayed on the surface of the conductive substrate to form an N-type graphene oxide layer; Heating the conductive substrate having the N-type graphene oxide layer to a second temperature, spraying the P-type graphene oxide precursor solution on the surface of the N-type graphene oxide layer to form a P-type graphene oxide layer; Preparing a silver electrode on the surface of the P-type graphene oxide layer to obtain the graphene oxide-based PN junction; Wherein, the first temperature is 120-300° C., and the second temperature is ≤ the first temperature.

7. The method for preparing a graphene oxide-based PN junction according to claim 6, characterized in that: In the precursor solution of the N-type graphene oxide, the content of the graphene oxide is 0.05 to 0.5 wt‰; and in the precursor solution of the P-type graphene oxide, the content of the graphene oxide is 0.05 to 0.5 wt‰; And / or, the organic solvent is selected from any one of methanol, ethanol, propanol, isopropanol or acetone, or a combination of at least two thereof.

8. The method for preparing a graphene oxide-based PN junction according to claim 6, characterized in that: In the preparation process of the N-type graphene oxide layer, the spraying adopts ultrasonic atomization spraying, and the specific parameter settings include: the nozzle reciprocates in a zigzag shape; the frequency range of the ultrasonic oscillation of the nozzle is 20000-100000Hz; the infusion rate range of the liquid pump is 0.05-0.5mL / min; the movement rate range of the nozzle is 2000-10000mm / min; the spraying thickness of a single layer is 10-50nm; the thickness of the N-type graphene oxide layer is made to a specified thickness by stacking multiple layers; And / or, during the preparation of the P-type graphene oxide layer, the spraying adopts ultrasonic atomization spraying, and the specific parameter settings include: the nozzle reciprocates in a zigzag shape; the frequency range of the ultrasonic oscillation of the nozzle is 20000~100000Hz; the infusion rate range of the liquid pump is 0.05~0.5mL / min; the movement rate range of the nozzle is 2000~10000mm / min; the single-layer spraying thickness is 10~50nm; and the P-type graphene oxide layer is made to a specified thickness by multi-layer superposition.

9. The method for preparing a graphene oxide-based PN junction according to claim 6, characterized in that: The silver electrode is prepared by printing silver paste using inkjet printing technology; And / or, the silver paste comprises, by mass percentage, 78-82% of silver powder, 8-12% of epoxy resin, 1-3% of anhydride curing agent, 4-6% of butyl acetate, and the remainder is a reactive diluent; And / or, the epoxy resin is selected from bisphenol A epoxy resin, and the number average molecular weight of the bisphenol A epoxy resin is 3000 to 7000; And / or, the anhydride curing agent is selected from any one or a combination of at least two of phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride or methyltetrahydrophthalic anhydride; And / or, the reactive diluent is selected from any one or a combination of at least two of acrylate, propenyl glycidyl ether, phenyl glycidyl ether or resorcinol bisglycidyl ether.

10. Use of the graphene oxide-based PN junction according to any one of claims 1 to 5 in preparing a semiconductor element.

Citation Information

Cited By

  • Photoelectric detector based on PIPD-graphene composite fiber

    CN121815878A