High-humidity tissue adhesion anti-swelling conductive hydrogel and preparation method thereof

Through the free radical polymerization of hydrophobic amino acid vinyl, hydrophilic and zwitter ionic units, a conductive hydrogel with high humidity tissue adhesion and swelling was constructed, which solved the adhesion of conductive hydrogels in high humidity or underwater environments. The problem of insufficient adhesion and swelling resistance has achieved firm bonding with biological tissues and stable signal transmission.

CN118892583AActive Publication Date: 2024-11-05XI AN JIAOTONG UNIV

Patent Information

Application Number
CN202410802621.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-05
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Conductive hydrogels have problems such as weak wet tissue adhesion and insufficient swelling resistance in high humidity or underwater environments, which are difficult to meet the application needs of tissue repair and physiological signal transmission.

Method used

Free radical polymerization of hydrophobic amino acid vinyl structural units, hydrophilic structural units and zwitterionic structural units is used to eliminate the interface hydration layer by hydrophobic groups, and non-covalent interaction with biological tissues is achieved, combining multiple hydrogen bonds and static electricity. Interactions to construct a conductive hydrogel with adhesion and swelling resistance to high humidity tissue.

Benefits of technology

It realizes a firm and long-term stable bond on wet biological tissue, has stable anti-swelling properties and conductivity, and can effectively transmit human physiological signals in high humidity or underwater environments. It is suitable for clinical hemostasis and bioflex sensing. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892583A_ABST
    Figure CN118892583A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polymer hydrogel, and particularly relates to high-humidity tissue adhesion anti-swelling conductive hydrogel. The high-humidity tissue adhesion anti-swelling conductive hydrogel comprises a hydrophobic amino acid vinyl structural unit, a hydrophilic structural unit and a zwitterionic structural unit. Through free radical polymerization of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer and the zwitterionic monomer, the conductive hydrogel with tissue matching property, biological safety, high-humidity tissue adhesion and swelling resistance is simply and efficiently constructed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer hydrogels, and in particular relates to a high-humidity tissue-adhesive and anti-swelling conductive hydrogel and a preparation method thereof. Background Art

[0002] Conductive hydrogels have shown broad application prospects in the fields of human-machine interface, implantable electronic devices, intelligent health diagnosis and treatment due to their advantages such as tissue similarity, good biocompatibility, and rapid response to various external stimuli. However, whether conducting hydrogels are used for physiological signal monitoring or defective tissue repair, they are inevitably interfered by different types of solutions (such as rain, sweat, body fluids, etc.) during use. First, the large number of hydrophilic functional groups on the traditional hydrogel polymer skeleton will cause the hydrogel to absorb a large amount of water molecules when in contact with the solution, causing volume swelling, thereby significantly reducing the mechanical properties of the hydrogel; secondly, water molecules will interfere with the direct contact or chemical bonding between the hydrogel and the bonding substrate, reducing the bonding strength between the hydrogel and the adhesion interface, thereby increasing the risk of human-machine interface failure or tissue fluid leakage due to sensor debonding during use. Therefore, in order to protect the conductive hydrogel from interference from different types of solutions when used in a dynamic wet environment, it is crucial to synergistically enhance the anti-swelling properties of the hydrogel matrix and the wet tissue adhesion of the interface.

[0003] In order to meet application needs, in recent years, researchers have effectively improved the anti-swelling properties of hydrogels by encapsulating the surface of hydrogels, introducing hydrophobic functional groups, and combining multiple interactions to achieve the structural and functional stability of conductive hydrogels in underwater environments. Professor Chen Fei of Xi'an Jiaotong University and Professor Xu Bin of Northumbria University in the United Kingdom collaborated to modify the hydrophobic ester gel coating on the surface of conductive hydrogels to give them unique anti-swelling properties (Adv. Funct. Mater. 2022, 32, 2201396). Professor Gao Guanghui of Changchun University of Technology and his team introduced the hydrophobic monomer 2-methoxyethyl acrylate into a hydrophilic polymer network to construct a solvent-resistant conductive hydrogel that can be stably present in a variety of organic solvents without obvious volume swelling (ACS Nano 2020, 14, 13709-13717). Professor Lv Shaoyu of Lanzhou University and his team copolymerized zwitterionic monomers with hydrophobic monomers hydroxyethyl methacrylate and combined them with polyvinyl alcohol. Based on multiple hydrogen bonds, electrostatic interactions, and double network structures, they designed an anti-swelling conductive hydrogel that can be used for underwater motion monitoring (Adv. Funct. Mater. 2022, 32, 2107404). However, the introduction of a large number of hydrophobic functional groups and the high cross-linking density of the hydrogel hinder the mobility of the polymer chains. Although it effectively prevents the penetration of water molecules into the gel, it also limits the migration of bonding functional groups to the bonding interface, weakening the wet bonding strength between the hydrogel and biological tissues. The lack of interfacial wet tissue bonding performance will seriously restrict the application potential of hydrogels for tissue repair or flexible sensing underwater or in physiological environments.

[0004] The surface of the hydrogel needs to have a large number of bonding functional groups to achieve multiple interactions between the hydrogel and the bonding matrix. However, the bonding functional groups usually form a hydration layer at the interface due to their strong hydrophilicity, which hinders the direct contact between the hydrogel and the bonding matrix and severely weakens the bonding strength at the interface. Therefore, in order to ensure that the conductive hydrogel forms a stable and strong bond on the wet and dynamic surface of biological tissue, it is necessary to eliminate the interference of the interfacial hydration layer on the interaction between the hydrogel and the target matrix as much as possible. It is worth noting that organisms in nature often contain ideas for solving this problem. Inspired by marine mussels, Professor Cao Yi of Nanjing University and his team combined the catechol structure with the polymer backbone. The catechol structure can effectively penetrate the interfacial hydration layer to interact with biological tissues, thereby constructing a hydrogel tape that can quickly form a strong bond with wet tissues (Nat. Commun. 2021, 12, 7156). Professor Yan Xuehai and his team from the Institute of Process Engineering of the Chinese Academy of Sciences integrated polydopamine nanoparticles with a catechol structure into the hydrogel network to give it stronger adhesion and lower impedance, which can avoid the interference of sweat during the monitoring of brain electrophysiological signals (Adv. Mater. 2023, 35, 2209606). Inspired by barnacles, Professor Gong Jianping and his team from Hokkaido University in Japan found that the copolymerization of adjacent sequences of cationic monomers and aromatic monomers gave the hydrogel the ability to quickly and reversibly adhere to negatively charged substrates in seawater (Adv. Funct. Mater. 2021, 31, 2009334). However, the catechol group is easily oxidized to quinone, resulting in a decrease in the number of phenolic hydroxyl groups, resulting in a decrease in bonding strength; in addition, the cation-π interaction depends on complex structural design and is easily affected by factors such as temperature, pH, and ion concentration. Therefore, it is a huge challenge to construct a conductive hydrogel with long-term stability and high-humidity tissue adhesion and anti-swelling properties through a simple and effective method. Summary of the invention

[0005] In view of the problem in the prior art that conductive hydrogels have weak wet tissue adhesion and insufficient anti-swelling performance, making it difficult to meet the application requirements of tissue repair or stable transmission of various physiological signals of the human body in high humidity or underwater environments, the present invention provides a conductive hydrogel with high wet tissue adhesion and anti-swelling properties.

[0006] The high-humidity tissue-adhesive and anti-swelling conductive hydrogel comprises a hydrophobic amino acid vinyl structural unit, a hydrophilic structural unit and a zwitterionic structural unit.

[0007] Furthermore, the quantitative ratio of the hydrophobic amino acid vinyl structural unit to the hydrophilic structural unit is 1:(8-20).

[0008] Furthermore, the quantitative ratio of the hydrophobic amino acid vinyl structural unit to the zwitterionic structural unit is 1:(0.9-3).

[0009] Further, the hydrophobic amino acid vinyl monomer corresponding to the hydrophobic amino acid vinyl structural unit is selected from one or more of N-acryloylalanine, N-acryloylvaline, N-acryloylphenylalanine, N-acryloylleucine, N-acryloylisoleucine, N-acryloyltryptophan, N-acryloylmethionine, N-acryloylalaninamide, N-acryloylvalinamide and N-acryloylphenylalanamide;

[0010] The hydrophilic monomer corresponding to the hydrophilic structural unit is selected from one or more of acrylic acid, methacrylic acid, 2-hydroxyethyl acrylic acid, hydroxyethyl methacrylate, acrylamide, N-trihydroxymethyl methacrylamide, N,N-dimethylacrylamide, N-hydroxyethyl acrylamide, 1-vinyl-2-pyrrolidone, N-acryloyl aspartic acid, N-acryloyl glutamic acid, N-acryloyl glycine, N-acryloyl tyrosine, N-acryloyl serine, N-acryloyl threonine and N-acryloyl glutamine;

[0011] The zwitterionic monomer corresponding to the zwitterionic structural unit is selected from one or more of 2-methacryloyloxyethyl phosphorylcholine, 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propionate, [3-(methacryloylamino)propyl]dimethyl(3-thiopropyl)ammonium hydroxide and [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide.

[0012] The invention also provides a method for preparing the high-humidity tissue-adhesive and anti-swelling conductive hydrogel.

[0013] The preparation method of the high-humidity tissue-adhesive anti-swelling conductive hydrogel comprises the following steps:

[0014] S1: fully dissolving the hydrophobic amino acid vinyl monomer, the hydrophilic monomer and the zwitterionic monomer in an aqueous solution to obtain a colorless transparent mixed solution;

[0015] S2: At room temperature, add initiator and initiator accelerator and mix them evenly to complete free radical polymerization;

[0016] S3: Soaking the polymer in deionized water to obtain the high-humidity tissue-adhesive and anti-swelling conductive hydrogel.

[0017] Further, the total concentration of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer is 4.4 to 8.8 mol / L;

[0018] The concentration of the zwitterionic monomer is 0.2-1.8 mol / L.

[0019] Further, the initiator is selected from one or more of potassium persulfate, ammonium persulfate and azobisisobutylimidazoline hydrochloride;

[0020] The initiator promoter is N,N,N',N'-tetramethylethylenediamine.

[0021] Furthermore, the added amount of the initiator is 0.5-2% of the total mass of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer and the zwitterionic monomer;

[0022] The added amount of the initiator accelerator is 0 to 30% of the mass of the initiator.

[0023] Further, in step S1, the method of sufficient dissolution is selected from one or more of heating, ultrasound and vortex oscillation;

[0024] In step S2, the polymerization temperature is 20 to 80° C., and the polymerization reaction time is 2 to 12 hours;

[0025] In step S3, the soaking time is 21 to 24 hours.

[0026] Compared with the prior art, the high-humidity tissue-adhesive and anti-swelling conductive hydrogel provided by the present invention has the following advantages:

[0027] 1) The hydrogel provided by the present invention is convenient and quick to use, and has strong and stable tissue adhesion. It only needs to be pressed for 20 seconds at a stress of 5 kPa to form a firm and long-term stable bond with moist biological tissues, and the bonding interface is not disturbed by external water molecules; furthermore, the hydrogel also exhibits a firm and stable wet bonding behavior to various organ tissues in the body, including the heart, liver, arteries, lungs, stomach, etc., and has the application potential of rapid hemostasis and promotion of tissue repair;

[0028] 2) The hydrogel provided by the present invention has stable anti-swelling properties underwater. No matter it is immersed in a deionized water solution or a simulated seawater solution for 10 days, the mass and volume of the hydrogel will not change significantly;

[0029] 3) The hydrogel provided by the present invention has stable and effective underwater sensing capabilities. In an underwater environment, the hydrogel can not only monitor the changes in electrical signals generated by human joint movements, but can also be used to collect physiological signals such as human pulse, electrocardiogram, and electromyography, providing a new option for clinical use to replace traditional adhesive tape-type commercial electrodes.

[0030] 4) The hydrogel provided by the present invention has good biocompatibility. The hydrogel patch obtained by free radical polymerization of amino acid derivatives, hydrophilic monomers and zwitterionic monomers has excellent biocompatibility, which is conducive to clinical transformation and provides a new option for clinically replacing surgical sutures to achieve wound closure and rapid hemostasis. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a graph showing the wet bonding strength test results between the hydrogels provided in Examples 2, 5, 6, and 7 and pig skin.

[0032] Figure 2 This is a graph showing the test results of wet bonding strength and bonding interface toughness between the hydrogel provided in Example 2 and various pig tissues.

[0033] Figure 3 This is a graph showing the change in swelling rate of the hydrogel provided in Example 2 when immersed in deionized water and seawater solution.

[0034] Figure 4 This is a graph showing the results of testing the changes in electromyographic signals when a hydrogel electrode patch and a commercial electrode patch were attached to a human forearm and immersed in an aqueous solution. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings, but they should not be construed as limiting the applicable scope of the present invention.

[0036] In view of the shortcomings of the prior art, the present invention intends to adopt a strategy of synergistic enhancement of the hydrogel interface and the matrix to regulate the steric hindrance of the polymer side chain and the spatial effect of the hydrophilic and hydrophobic groups. Through the free radical polymerization of hydrophobic amino acid vinyl monomers, hydrophilic monomers and zwitterionic monomers, a conductive hydrogel with tissue matching, biosafety, high-humidity tissue adhesion and anti-swelling is simply and efficiently constructed.

[0037] The present invention provides a high-humidity tissue adhesive anti-swelling conductive hydrogel and a preparation method thereof. The present invention obtains a hydrogel by free radical polymerization of hydrophobic amino acid vinyl monomers, hydrophilic monomers and zwitterionic monomers in aqueous solution. When the hydrogel contacts with moist biological tissue, the hydrophobic effect of the hydrophobic group effectively removes the interfacial hydration layer, and then combines the non-covalent interaction of various hydrophilic groups with biological tissues to achieve rapid and firm adhesion with various biological tissues in a wet environment. At the same time, based on the hydrophobic effect and multiple hydrogen bonds and electrostatic interactions between molecules, the hydrogel has stable and durable underwater anti-swelling performance, and can effectively resist the infiltration of external water molecules in high humidity or underwater environments. In addition, due to the introduction of conductive functional groups such as carboxyl and sulfonic acid groups, the hydrogel has excellent conductivity and bioelectric signal sensing capabilities, and can stably transmit various physiological signals of the human body in high humidity or underwater environments. The hydrogel raw materials prepared by the present invention are cheap and easy to obtain, have excellent mechanical properties, good biocompatibility, and are conducive to clinical transformation, providing new options for applications in the fields of clinical emergency hemostasis, tissue damage repair, and biological flexible sensing.

[0038] The high-humidity tissue-adhesive and anti-swelling conductive hydrogel comprises a hydrophobic amino acid vinyl structural unit, a hydrophilic structural unit and a zwitterionic structural unit.

[0039] In one embodiment, the ratio of the number of hydrophobic amino acid vinyl structural units to the number of hydrophilic structural units is 1:(8-20);

[0040] The quantitative ratio of the hydrophobic amino acid vinyl structural units to the zwitterionic structural units is 1:(0.9-3).

[0041] In one embodiment, the hydrophobic amino acid vinyl monomer corresponding to the hydrophobic amino acid vinyl structural unit is selected from one or more of N-acryloylalanine (AL), N-acryloylvaline (AV), N-acryloylphenylalanine (APA), N-acryloylleucine (ALE), N-acryloylisoleucine (AIL), N-acryloyltryptophan (ATP), N-acryloylmethionine (AMT), N-acryloylalaninamide (ALN), N-acryloylvalinamide (AVN) and N-acryloylphenylpropionamide (APN).

[0042] In one embodiment, the hydrophilic monomer corresponding to the hydrophilic structural unit is selected from one or more of acrylic acid (AA), methacrylic acid (MAA), 2-hydroxyethyl acrylate (HEA), hydroxyethyl methacrylate (HEMA), acrylamide (AM), N-trihydroxymethyl methacrylamide (THMA), N,N-dimethylacrylamide (DMA), N-hydroxyethyl acrylamide (HEAA), 1-vinyl-2-pyrrolidone (NVP), N-acryloyl aspartic acid (AASP), N-acryloyl glutamic acid (AGLU), N-acryloyl glycine (AG), N-acryloyl tyrosine (AT), N-acryloyl serine (AS), N-acryloyl threonine (AT) and N-acryloyl glutamine (AGT).

[0043] In one embodiment, the zwitterionic monomer corresponding to the zwitterionic structural unit is selected from one or more of 2-methacryloyloxyethylphosphorylcholine (MPC), 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propionate (CBMA), [3-(methacrylamido)propyl]dimethyl(3-thiopropyl)ammonium hydroxide (SBAA) and [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide (SBMA).

[0044] The preparation method of the high-humidity tissue-adhesive anti-swelling conductive hydrogel comprises the following steps:

[0045] S1: fully dissolving a hydrophobic amino acid vinyl monomer, a hydrophilic monomer and a zwitterionic monomer in an aqueous solution to obtain a colorless transparent mixed solution;

[0046] S2: At room temperature, add initiator and initiator accelerator and mix them evenly to complete free radical polymerization;

[0047] S3: Soaking the polymer in deionized water to obtain the high-humidity tissue-adhesive and anti-swelling conductive hydrogel.

[0048] In one embodiment, the total concentration of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer is 4.4 to 8.8 mol / L;

[0049] The concentration of the zwitterionic unit monomer is 0.2-1.8 mol / L.

[0050] In one embodiment, the concentration of the zwitterionic monomer is 0.2 to 1.8 mol / L;

[0051] In one embodiment, the initiator is selected from one or more of potassium persulfate, ammonium persulfate and azobisisobutylimidazoline hydrochloride;

[0052] The initiator promoter is N,N,N',N'-tetramethylethylenediamine.

[0053] In one embodiment, the added amount of the initiator is 0.5-2% of the total mass of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer and the zwitterionic monomer;

[0054] The added amount of the initiator accelerator is 0 to 30% of the mass of the initiator.

[0055] In one embodiment, in step S1, the method of sufficient dissolution is selected from one or more of heating, ultrasound and vortex oscillation;

[0056] In step S2, the polymerization temperature is 20 to 80° C., and the polymerization reaction time is 2 to 12 hours;

[0057] In step S3, the soaking time is 21 to 24 hours.

[0058] Examples 1-19 are provided based on the preparation method of the high-humidity tissue-adhesive and anti-swelling conductive hydrogel provided above.

[0059] The hydrophobic amino acid vinyl monomer mentioned in the present invention is obtained according to the method described in the references Biomacromolecules 2021, 22, 1297-1304; Sci. Adv. 2023, 9, eadg4031.

[0060] Example 1: P(APA 0.7 -AA 7.0 -SBMA 0.6 )

[0061] Free radical copolymerization of APA, AA and SBMA monomers: 153 mg APA, 504 mg AA and 168 mg SBMA were dissolved in 1 mL deionized water by heating at 60 °C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 0.6 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 8.3 mg ammonium persulfate was added as an initiator, 2.5 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 °C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0062] Example 2: P(APA 0.7 -AA 7.0 -SBMA 1.2 )

[0063] Free radical copolymerization of APA, AA and SBMA monomers: 153 mg APA, 504 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.9 mg ammonium persulfate was added as an initiator, 3.0 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0064] Example 3: P(APA 0.7 -AA 7.0 -SBMA 1.8 )

[0065] Free radical copolymerization of APA, AA and SBMA monomers: 153 mg APA, 504 mg AA and 503 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.8 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 11.6 mg ammonium persulfate was added as an initiator, 3.5 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0066] Example 4: P(APA 0.4 -AA 4.0 -SBMA 1.2 )

[0067] Free radical copolymerization of APA, AA and SBMA monomers: 88 mg APA, 288 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60°C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.4 mol / L, the concentration of AA was 4.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 7.1 mg ammonium persulfate was added as an initiator, 2.1 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60°C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0068] Example 5: P(APA 0.5 -AA 5.0 -SBMA 1.2 )

[0069] Free radical copolymerization of APA, AA and SBMA monomers: 110 mg APA, 360 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.5 mol / L, the concentration of AA was 5.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 8.0 mg ammonium persulfate was added as an initiator, 2.4 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0070] Example 6: P(APA 0.6 -AA 6.0 -SBMA 1.2 )

[0071] Free radical copolymerization of APA, AA and SBMA monomers: 131 mg APA, 432 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 °C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.6 mol / L, the concentration of AA was 6.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.0 mg ammonium persulfate was added as an initiator, 2.7 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 °C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0072] Example 7: P(APA 0.8 -AA 8.0 -SBMA 1.2 )

[0073] Free radical copolymerization of APA, AA and SBMA monomers: 175 mg APA, 576 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.8 mol / L, the concentration of AA was 8.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 10.9 mg ammonium persulfate was added as an initiator, 3.3 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0074] Example 8: P(AL 0.7 -AA 7.0 -SBMA 1.2 )

[0075] Free radical copolymerization of AL, AA and SBMA monomers: 100 mg AL, 504 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of AL was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.4 mg ammonium persulfate was added as an initiator, 2.8 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0076] Example 9: P(AV 0.7 -AA 7.0 -SBMA 1.2 )

[0077] Free radical copolymerization of AV, AA and SBMA monomers: 120 mg AV, 504 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of AV was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.6 mg ammonium persulfate was added as an initiator, 2.9 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0078] Example 10: P(ALE 0.7 -AA 7.0 -SBMA 1.2 )

[0079] Free radical copolymerization of ALE, AA and SBMA monomers: 130 mg ALE, 504 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of ALE was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.7 mg ammonium persulfate was added as an initiator, 2.9 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0080] Example 11: P(AIL 0.7 -AA 7.0 -SBMA 1.2 )

[0081] Free radical copolymerization of AIL, AA and SBMA monomers: 130 mg AIL, 504 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of AIL was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.7 mg ammonium persulfate was added as an initiator, 2.9 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0082] Example 12: P(ATP 0.7 -AA 7.0 -SBMA 1.2 )

[0083] Free radical copolymerization with ATP, AA and SBMA monomers: 181 mg ATP, 504 mg AA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60°C, ultrasound, vortex oscillation, etc., so that the concentration of ATP was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 10.2 mg ammonium persulfate was added as an initiator, 3.1 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator, and the mixture was evenly mixed and placed in an oven at 60°C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0084] Example 13: P(APA 0.7 -MAA 7.0 -SBMA 1.2 )

[0085] Free radical copolymerization of APA, MAA and SBMA monomers: 153 mg APA, 603 mg MAA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of MAA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 10.9 mg ammonium persulfate was added as an initiator, 3.3 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0086] Example 14: P(APA 0.7 -HEAA 7.0 -SBMA 1.2 )

[0087] Free radical copolymerization of APA, HEAA and SBMA monomers: 153 mg APA, 806 mg HEAA and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of HEAA was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 12.9 mg ammonium persulfate was added as an initiator, 3.9 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0088] Example 15: P(APA 0.7 -AG 7.0 -SBMA 1.2 )

[0089] Free radical copolymerization of APA, AG and SBMA monomers: 153 mg APA, 904 mg AG and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AG was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 13.9 mg ammonium persulfate was added as an initiator, 4.2 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0090] Example 16: P(APA 0.7 -AASP 7.0 -SBMA 1.2 )

[0091] Free radical copolymerization of APA, AASP and SBMA monomers: 153 mg APA, 1310 mg AASP and 335 mg SBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AASP was 7.0 mol / L, and the concentration of SBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 18.0 mg ammonium persulfate was added as an initiator, 5.4 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0092] Example 17: P(APA 0.7 -AA 7.0 -MPC 1.2 )

[0093] Free radical copolymerization of APA, AA and MPC monomers: 153 mg APA, 504 mg AA and 354 mg MPC were dissolved in 1 mL deionized water by heating at 60 °C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of MPC was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 10.1 mg ammonium persulfate was added as an initiator, 3.0 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator accelerator, and the mixture was evenly mixed and placed in an oven at 60 °C for 3 h to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 h to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0094] Example 18: P(APA 0.7 -AA 7.0 -CBMA 1.2 )

[0095] Free radical copolymerization of APA, AA and CBMA monomers: 153 mg APA, 504 mg AA and 275 mg CBMA were dissolved in 1 mL deionized water by heating at 60 ° C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of CBMA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 9.3 mg ammonium persulfate was added as an initiator, 2.8 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60 ° C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0096] Example 19: P(APA 0.7 -AA 7.0 -SBAA 1.2 )

[0097] Free radical copolymerization of APA, AA and SBAA monomers: 153 mg APA, 504 mg AA and 351 mg SBAA were dissolved in 1 mL deionized water by heating at 60°C, ultrasound, vortex oscillation, etc., so that the concentration of APA was 0.7 mol / L, the concentration of AA was 7.0 mol / L, and the concentration of SBAA was 1.2 mol / L. After complete dissolution, the mixed solution was cooled to room temperature, 10.1 mg ammonium persulfate was added as an initiator, 3.0 mg N,N,N',N'-tetramethylethylenediamine was added as an initiator promoter, and the mixture was evenly mixed and placed in an oven at 60°C for 3 hours to initially obtain a hydrogel. The hydrogel was soaked in deionized water for 24 hours to finally obtain a purified high-humidity tissue adhesion anti-swelling conductive hydrogel.

[0098] Effect test:

[0099] Figure 1 The wet bonding strength between the hydrogels provided in Examples 2, 5, 6, and 7 and pig skin is shown. As the content of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer increases, the wet bonding strength gradually increases. The wet bonding strength of the hydrogel provided in Example 7 is as high as 93 kPa, which has obvious advantages over the catechol-based hydrogel patch (Adv. Mater. 2023, 35, 2209606; Biomaterials 2023, 301, 122240).

[0100] Figure 2 It was demonstrated that the hydrogel provided in Example 2 exhibited strong wet bonding strength and firm bonding interface toughness with different pig tissues (including liver, lung, heart, stomach, artery, and skin).

[0101] Figure 3 The changes in swelling rate of the hydrogel provided in Example 2 when immersed in deionized water and simulated seawater solution are shown. The hydrogel has anti-swelling properties in aqueous solution, and after immersion for 10 days, the swelling rate of the hydrogel is less than 4%; further, the hydrogel has anti-dehydration properties in the simulated seawater solution, and after immersion for 10 days, the water loss rate of the hydrogel is less than 1%.

[0102] Figure 4 A comparative test of collecting electromyographic signals by attaching a hydrogel electrode patch modified with the hydrogel provided in Example 2 and an unmodified commercial electrode patch (Hangzhou Xunda Radio Equipment Co., Ltd.) to a human forearm and immersing it in an aqueous solution is shown. The hydrogel electrode patch is obtained by replacing the adhesive tape and the conductive hydrogel of the commercial electrode patch with the hydrogel provided in Example 2. The weight lifted by the forearm in the test is 2.5 kg. During the test, the signal output of the hydrogel electrode patch is stable and the signal-to-noise ratio is always maintained at a high level, while the signal of the commercial electrode patch is significantly attenuated and ultimately presents a lower signal-to-noise ratio. This result shows that the hydrogel provided by the present invention has stable and durable underwater conductivity and sensing capabilities.

[0103] The high-humidity tissue adhesion and anti-swelling conductive hydrogel provided by the present invention can achieve rapid and firm adhesion when in contact with moist biological tissue. At the same time, the hydrogel has stable and durable underwater anti-swelling performance, and can effectively resist the infiltration of external water molecules in high humidity or underwater environments. In addition, the hydrogel has long-term stable conductivity and bioelectric signal sensing capabilities, and can stably transmit a variety of physiological signals of the human body in high humidity or underwater environments. The hydrogel raw materials prepared by the present invention are cheap and easy to obtain, have excellent mechanical properties, and good biocompatibility, which is conducive to clinical transformation and provides new options for applications in the fields of clinical emergency hemostasis, tissue damage repair, and biological flexible sensing.

Claims

1. A high-humidity tissue-adhesive and anti-swelling conductive hydrogel, characterized in that: It includes hydrophobic amino acid vinyl structural units, hydrophilic structural units and zwitterionic structural units.

2. The high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 1, characterized in that: The quantitative ratio of the hydrophobic amino acid vinyl structural unit to the hydrophilic structural unit is 1:(8-20).

3. The high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 2, characterized in that: The quantity ratio of the hydrophobic amino acid vinyl structural unit to the zwitterionic structural unit is 1:(0.9-3).

4. The high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 1, characterized in that: The hydrophobic amino acid vinyl monomer corresponding to the hydrophobic amino acid vinyl structural unit is selected from one or more of N-acryloylalanine, N-acryloylvaline, N-acryloylphenylalanine, N-acryloylleucine, N-acryloylisoleucine, N-acryloyltryptophan, N-acryloylmethionine, N-acryloylalaninamide, N-acryloylvalinamide and N-acryloylphenylalanamide; The hydrophilic monomer corresponding to the hydrophilic structural unit is selected from one or more of acrylic acid, methacrylic acid, 2-hydroxyethyl acrylic acid, hydroxyethyl methacrylate, acrylamide, N-trihydroxymethyl methacrylamide, N,N-dimethylacrylamide, N-hydroxyethyl acrylamide, 1-vinyl-2-pyrrolidone, N-acryloyl aspartic acid, N-acryloyl glutamic acid, N-acryloyl glycine, N-acryloyl tyrosine, N-acryloyl serine, N-acryloyl threonine and N-acryloyl glutamine; The zwitterionic monomer corresponding to the zwitterionic structural unit is selected from one or more of 2-methacryloyloxyethyl phosphorylcholine, 3-[[2-(methacryloyloxy)ethyl]dimethylammonium]propionate, [3-(methacryloylamino)propyl]dimethyl(3-thiopropyl)ammonium hydroxide and [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfonatepropyl)ammonium hydroxide.

5. A method for preparing the high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claims 1-4, characterized in that: The following steps are involved: S1: fully dissolving a hydrophobic amino acid vinyl monomer, a hydrophilic monomer and a zwitterionic monomer in an aqueous solution to obtain a colorless transparent mixed solution; S2: At room temperature, add initiator and initiator accelerator and mix them evenly to complete free radical polymerization; S3: Soaking the polymer in deionized water to obtain the high-humidity tissue-adhesive and anti-swelling conductive hydrogel.

6. The method for preparing the high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 5, characterized in that: The total concentration of the hydrophobic amino acid vinyl monomer and the hydrophilic monomer is 4.4-8.8 mol / L; The concentration of the zwitterionic unit monomer is 0.2-1.8 mol / L.

7. The method for preparing the high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 6, characterized in that: The initiator is selected from one or more of potassium persulfate, ammonium persulfate and azobisisobutylimidazoline hydrochloride; The initiator promoter is N,N,N',N'-tetramethylethylenediamine.

8. The method for preparing the high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 6, characterized in that: The added amount of the initiator is 0.5-2% of the total mass of the hydrophobic amino acid vinyl monomer, the hydrophilic monomer and the zwitterionic monomer; The added amount of the initiator accelerator is 0 to 30% of the mass of the initiator.

9. The method for preparing the high-humidity tissue-adhesive and anti-swelling conductive hydrogel according to claim 6, characterized in that: In step S1, the method of sufficient dissolution is selected from one or more of heating, ultrasound and vortex oscillation; In step S2, the polymerization temperature is 20 to 80° C., and the polymerization reaction time is 2 to 12 hours; In step S3, the soaking time is 21 to 24 hours.

Citation Information

Patent Citations

  • Anti-swelling anti-adhesion hydrogel as well as preparation method and application thereof

    CN112708075A

  • Preparation method and application of anti-swelling zwitterionic hydrogel sensing material with controllable rehydration and high strain sensitivity

    CN113968981A

  • Hydrogel with different adhesion properties on two sides as well as preparation method and application of hydrogel

    CN114106232A

  • Biological tissue adhesive capable of being instantly adhered when encountering water and preparation method of biological tissue adhesive

    CN115612014A

  • Anti-swelling adhesion ionic gel as well as preparation method and application thereof

    CN115894793A

Cited By

  • Self-adaptive Janus supramolecular hydrogel, preparation method and application of self-adaptive Janus supramolecular hydrogel as wet tissue surface adhesive

    CN119552318A

  • An adaptive Janus supramolecular hydrogel, preparation method and application thereof as a wet tissue surface adhesive