Preparation method of bimetallic oxide functionalized double-layer mesoporous composite adsorbent and defluorination application of bimetallic oxide functionalized double-layer mesoporous composite adsorbent

By fixing lysozyme on a double-layer mesoporous hollow carbon sphere and generating zirconium and lanthanum bimetal oxides to form functional adsorbents, the problems of low fluorine removal efficiency and easy leaching of adsorbents in the prior art are solved, and the problem of low fluorine removal efficiency and easy leaching of adsorbents in the prior art is achieved. High-efficiency fluorine removal effect under acidic conditions.

CN118892815AActive Publication Date: 2024-11-05JIANGSU UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411316528.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-05
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

The existing fluorine-removing adsorbents are inefficient under acidic conditions and are prone to leaching metal hydroxides during adsorption, and there are major resistance problems when collecting and dynamic separation of nanometal oxide adsorbents.

Method used

The double-layer mesoporous hollow carbon sphere is used to load bimetallic hydroxide composite adsorbent, and lysozyme is fixed by physical adsorption and zirconium and lanthanum bimetallic oxides are generated under alkaline conditions to form a functionalized bimetallic mesoporous composite adsorbent. Used for efficient fluorine removal under acidic conditions.

Benefits of technology

It achieves efficient fluorine removal in an acidic environment, and the adsorbent has a large specific surface area and uniform adsorption site distribution, which improves the deep adsorption and separation effect of fluoride ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892815A_ABST
    Figure CN118892815A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of adsorption separation functional materials, and discloses a preparation method and defluorination application of a bimetallic oxide functionalized double-layer mesoporous composite adsorbent. According to the invention, phenolic resin and tetraethyl orthosilicate have different hydrolysis rates under an alkaline condition, and carbon spheres with a double-layer mesoporous hollow structure are synthesized under the condition of no assistance of a surfactant; then the lysozyme is fixed in the carbon spheres through physical adsorption, and rich and uniformly distributed groups on the surface of the lysozyme provide conditions for functional modification of the double-metal hydroxide. Mixing a metal salt solution with the enzyme-grafted carbon spheres at normal temperature, and then adding sodium hydroxide to generate zirconium and lanthanum double-metal hydroxides in situ under an alkaline condition, thereby obtaining the double-layer mesoporous double-metal oxide carbon spheres. The carbon spheres with the double-layer mesoporous hollow structure are combined with the double-metal oxide, so that the composite material still has excellent defluorination performance under the acidic condition, adsorption equilibrium is achieved within 30 minutes, and the adsorption capacity is 110 mg.g <-1 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparation of adsorption and separation functional materials, and relates to the preparation of metal hydroxide adsorbents, and in particular to a preparation method of a double-layer mesoporous material grown bimetallic oxide composite adsorbent, and the high-efficiency fluorine removal application of the adsorbent. Background Art

[0002] Fluorine (F) is one of the trace elements required by the human body. It is mainly found in human teeth and bones. Appropriate intake of fluorine can prevent tooth decay and promote bone development. However, long-term intake of high concentrations of fluorine can cause fluorosis, skeletal fluorosis and other diseases. With the rapid development of new energy batteries, photovoltaics, phosphate fertilizers and other industries, the probability of groundwater being contaminated by fluorine is also increasing. Studies have shown that one-third of rivers and 60% of groundwater fluoride pollution in my country is mainly caused by the discharge of industrial wastewater. Fluorine elements discharged into the environment without proper treatment will cause local drinking water fluoride to exceed the standard, threatening human health. Therefore, it is of great significance to explore efficient fluoride removal methods and make them meet emission standards. Among them, the adsorption method has the advantages of simple operation, low cost, and a wide range of material sources and is widely used in fluoride removal. The existing defluorination adsorbents include metal oxides, biomass-based materials, carbon-based materials, etc. Carbon-based materials have the advantages of large specific surface area and multi-mesoporous structure, but their adsorption effect on fluoride ions is weak. Metal hydroxides can form stable metal-ligand interactions with fluorides due to their strong alkalinity and electronic potential, and have a strong affinity for fluoride ions. However, metal hydroxides are easily leached during the adsorption process and show great resistance due to the pressure drop in the fixed bed column.

[0003] In order to achieve efficient fluorine removal under acidic conditions and solve the above problems, metal hydroxides can be loaded on porous carbon materials. However, how to grow metal hydroxides on mesoporous carbon spheres that lack rich functional groups is a new difficulty that needs to be solved. Lysozyme has the advantages of wide sources, stable chemical properties and certain antibacterial properties, and is a bridge between metal hydroxides and double-layer mesoporous hollow carbon spheres. Double-layer mesoporous carbon spheres with high specific surface area and mesoporous structure fix lysozyme on carbon spheres by physical adsorption. The rich functional groups on the surface of lysozyme provide a beneficial platform for the chelation of metal zirconium ions and lanthanum ions, and double metal hydroxides are generated in situ under alkaline conditions. Zirconium and lanthanum double metal hydroxides can show excellent fluorine removal performance under acidic conditions. The prepared double metal hydroxide carbon spheres still have a large specific surface area, and there are adsorption sites distributed in the inner and outer layers of the carbon spheres, laying the foundation for efficient fluorine removal. At present, there are no related reports. Summary of the invention

[0004] In order to solve the problems in the prior art that nano-metal oxide adsorbents are difficult to collect and easily cause large column pressure during dynamic separation, and to achieve efficient fluorine removal under acidic conditions, the present invention has established a preparation method for a double-layer mesoporous hollow material loaded with double metal hydroxide composite adsorbent. First, a hollow carbon sphere (MHCS) with a double-layer mesoporous structure was prepared, and then enzyme-attached carbon spheres (enzyme-MHCS) were prepared by physically adsorbing and fixing lysozyme. Zirconium and lanthanum metal ion solutions were mixed with enzyme-attached carbon spheres and metal hydroxides were generated in situ under alkaline conditions to prepare a double-metal oxide functionalized double-layer mesoporous composite adsorbent (Zr-La-MHCS), and the defluorination application of the adsorbent was explored.

[0005] A method for preparing a bimetallic oxide functionalized double-layer mesoporous composite adsorbent comprises the following steps:

[0006] (1) Preparation of double-layer mesoporous hollow carbon spheres (MHCS)

[0007] Tetraethyl orthosilicate (TEOS), resorcinol and formalin were added to a solution consisting of aqueous ammonia solution, deionized water and ethanol, and stirred vigorously at room temperature for t1, then TEOS was added and stirring continued for t2, and finally placed in a polytetrafluoroethylene-lined autoclave for further hydrothermal treatment, the solid product was collected by centrifugation and dried overnight, and MHCS nanoparticles were obtained after carbonization under N2 atmosphere and removal of the silica template by hydrofluoric acid etching.

[0008] (2) Preparation of enzyme-MHCS

[0009] Take lysozyme LYM and add it to deionized water to prepare a lysozyme solution, add the MHCS nanoparticles prepared in step (1) to the lysozyme solution, and fix LYM on the MHCS nanoparticles by physical adsorption; then put the mixed solution into a centrifuge tube, place it on a shaker for adsorption and fixation, centrifuge, wash with deionized water, and freeze-dry for use, to obtain enzyme-MHCS carbon spheres.

[0010] (3) Preparation of double metal oxide functionalized double-layer mesoporous composite adsorbent (Zr-La-MHCS)

[0011] Lanthanum chloride LaCl3, zirconium oxychloride octahydrate ZrOCl2·8H2O and enzyme-MHCS were dispersed in HCl solution and stirred with a magnetic bar for a period of time to chelate the metal ions with the enzyme; then NaOH solution was added, the reaction was continued with stirring, centrifuged, washed with deionized water, and freeze-dried to obtain a double-metal oxide functionalized double-layer mesoporous composite adsorbent Zr-La-MHCS.

[0012] In the preferred disclosed example of the present invention, the double-layer mesoporous hollow carbon sphere (MHCS) of step (1) is synthesized according to the prior art (Self-Organized Mesostructured Hollow Carbon Nanoparticles via a Surfactant-Free Sequential Heterogeneous Nucleation Pathway Hongwei Zhang, Meihua Yu, Hao Song, Owen Noonan, Jun Zhang, Yannan Yang, Liang Zhou, and Chengzhong Yu Chemistry of Materials 2015 27(18), 6297-6304 DOI: 10.1021 / acs.chemmater.5b01993). The synthesis method used in the present invention is disclosed herein:

[0013] In step (1), the amount ratio of tetraethyl orthosilicate TEOS, resorcinol, formalin, ammonia solution, deionized water, ethanol and TEOS is 2.8mL:0.4g:0.56mL:3.0mL:10mL:70mL:1.5mL; wherein the concentration of formalin is 37wt% and the concentration of ammonia solution is 28wt%;

[0014] The stirring time t1 is 6 hours, and the stirring time t2 is 24 hours;

[0015] The temperature of the hydrothermal treatment was 100°C and the time was 24 hours;

[0016] The carbonization temperature was 700°C and the concentration of hydrofluoric acid was 5%.

[0017] In step (2), the ratio of lysozyme to deionized water is 30-60 mg: 30-50 mL.

[0018] Preferably, the usage ratio of LYM and deionized water is 30 mg:40 mL.

[0019] In step (2), the mass volume ratio of MHCS to lysozyme aqueous solution is 30-60 mg:30-50 mL.

[0020] Preferably, the mass volume ratio of MHCS to the lysozyme aqueous solution is 20.0 mg:40 mL.

[0021] In step (2), the adsorption fixation time is 12.0 h.

[0022] In step (3), the mass volume ratio of LaCl3, ZrOCl2·8H2O, enzyme-MHCS and HCl solution is 20-50 mg: 20-50 mg: 20-50 mg: 20-50 mL.

[0023] Preferably, the mass volume ratio of LaCl3, ZrOCl2·8H2O, enzyme-MHCS and HCl solution is 25 mg:25 mg:50 mg:30 mL, wherein the concentration of HCl solution is 0.1M.

[0024] In step (3), the volume ratio of NaOH solution to HCl solution is 10-20 mL:20-50 mL, wherein the concentration of NaOH solution is 1 M.

[0025] In step (3), the stirring reaction time is 2.5 hours at room temperature.

[0026] The bimetallic oxide functionalized double-layer mesoporous composite adsorbent prepared by the present invention is used for deep adsorption and separation of fluoride ions. In an environment of 25° C., 2.0 mg of the prepared adsorbent (Zr-La-MHCS) is placed in 9.0 mL of 50 mg / L fluoride ion solution for adsorption. After 3.0 hours, the adsorbed solution is taken out and the concentration is tested.

[0027] Adsorption capacity calculation formula:

[0028] Where C0 (mg L -1 ) and C e (mg / L) are the initial concentration and equilibrium concentration of fluoride ions, respectively. V (mL) is the volume of the test solution, and m (g) is the mass of the adsorbent.

[0029] The adsorption performance evaluation of the present invention is carried out according to the following method:

[0030] Adsorption experiment: 2.0 mg of the adsorbent (Zr-La-MHCS) prepared according to the method of the present invention was added to 9.0 mL of the test solution with an initial pH of 2 to 8 (concentration value of 50 mg L -1 ), the residual fluoride ion content after adsorption was determined by ion chromatography, and the adsorption capacity was calculated based on the results; after saturated adsorption, the adsorption effect of Zr-La-MHCS was studied by the adsorption amount at different concentrations and temperatures; kinetic adsorption was carried out under the same conditions using different adsorbents; and the adsorption effect of Zr-La-MHCS in the presence of competing ions was studied by changing the impurity ion concentration.

[0031] The beneficial effects of the present invention are:

[0032] The present invention combines high specific surface area carbon balls with mesoporous hollow structures with double metal hydroxides. Double metal zirconium and lanthanum hydroxides grow on the inner and outer layers of the carbon balls. The abundant adsorption sites can be used for efficient fluorine removal, and a good fluorine removal effect is shown in an acidic environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 SEM and TEM images of MHCS (a, e), enzyme-MHCS (b, f) and Zr-La-MHCS (c, g) prepared in Example 1;

[0034] Figure 2 BET diagram of original carbon sphere MHCS and enzyme-MHCS;

[0035] Figure 3 The effect of different pH conditions on the adsorption capacity of Zr-La-MHCS and fluoride ions and the corresponding zeta potential;

[0036] Figure 4 Adsorption kinetics and model fitting curves for different adsorption materials;

[0037] Figure 5 The adsorption isotherm and model fitting curve of Zr-La-MHCS;

[0038] Figure 6 This is a comparison chart of fluorine adsorption and removal by Zr-La-MHCS in the presence of competing ions. DETAILED DESCRIPTION

[0039] The present invention is described in detail below in conjunction with the embodiments so that those skilled in the art can better understand the present invention, but the present invention is not limited to the following embodiments.

[0040] Example 1

[0041] (1) Preparation of MHCS particles with a size of 200 nm by polymerization

[0042] Tetraethyl orthosilicate (TEOS, 2.8 mL), resorcinol (0.4 g) and formalin (37 wt%, 0.56 mL) were added to a solution consisting of aqueous ammonia solution (3.0 mL, 28 wt%), deionized water (10 mL) and ethanol (70 mL), stirred vigorously for 6 hours at room temperature, then 1.5 mL of TEOS was added and stirred for 24 hours, and the mixture was further hydrothermally treated in a polytetrafluoroethylene-lined autoclave at 100 ° C for 24 hours. The solid product was collected by centrifugation and dried at 50 ° C overnight. After carbonization at 700 ° C in N2 atmosphere and removal of the silica template by hydrofluoric acid (HF, 5%) etching, MHCS was obtained.

[0043] Figure 1 a and e are SEM and TEM images of MHCS particles. It can be seen from the figures that the particles are evenly distributed and uniform in size, proving the successful preparation of double-layer mesoporous hollow carbon spheres.

[0044] (2) Preparation of enzyme-MHCS

[0045] Take 30 mg of lysozyme (LYM) and add it to 50 mL of deionized water to prepare a solution. Take 50 mg of MHCS nanoparticles prepared in step (1) and add them to the lysozyme solution to fix LYM on the MHCS nanoparticles by physical adsorption. Put the prepared solution into a centrifuge tube, place it on a shaker for adsorption and fixation for 12 hours, centrifuge, wash with deionized water, and freeze-dry for use. Obtain enzyme-MHCS carbon spheres.

[0046] Figure 1 Figures b and f are SEM and TEM images of the enzyme-attached carbon spheres. It can be seen from the figures that the shell of the carbon spheres is thickened and the surface becomes rough, which proves the successful immobilization of lysozyme.

[0047] Figure 2 BET characterization diagrams of MHCS and enzyme-MHCS, proving that their structures are mesoporous.

[0048] (3) Preparation of Zr-La-MHCS

[0049] 25 mg of lanthanum chloride (LaCl3), 25 mg of zirconium oxychloride octahydrate (ZrOCl2·8H2O) and 30 mg of the enzyme-linked carbon spheres prepared in step 2 were dispersed in 30 mL of HCl (0.1 M) solution and stirred with a magnetic bar for 2.5 h at room temperature to chelate the metal ions with the enzyme. 14 mL of NaOH (1 M) solution was added to the solution in step 1 and stirred for 2.5 h. The product was washed with deionized water and collected by centrifugation. After freeze drying, a double metal oxide functionalized double-layer mesoporous composite adsorbent (Zr-La-MHCS) was obtained.

[0050] Figure 1 Figures c and g are the SEM and TEM images of the enzyme-linked carbon spheres. It can be seen from the figures that particulate matter is generated in the inner and outer layers of the carbon spheres, and metal hydroxides grow evenly on the surface of the carbon spheres, which proves that the bimetallic oxides are generated in situ on the carbon spheres.

[0051] Example 2

[0052] The operations of steps (1) and (3) are the same as those of steps (1) and (3) of Example 1.

[0053] (2) Preparation of enzyme-MHCS

[0054] Take 30 mg of lysozyme (LYM) and add it to 40 mL of deionized water to prepare a solution. Take 50 mg of MHCS nanoparticles prepared in step (1) and add them to the enzyme solution to fix LYM on the MHCS nanoparticles by physical adsorption. Put the prepared solution into a centrifuge tube, place it on a shaker for adsorption and fixation for 12 hours, centrifuge, wash with deionized water, and freeze-dry for use. Obtain enzyme-MHCS carbon spheres.

[0055] Example 3

[0056] The operations of steps (1) and (3) are the same as those of steps (1) and (3) of Example 1.

[0057] (2) Preparation of enzyme-MHCS

[0058] Take 30 mg of lysozyme (LYM) and add it to 40 mL of deionized water to prepare a solution. Take 50 mg of MHCS nanoparticles prepared in step (1) and add them to the enzyme solution to fix LYM on the MHCS nanoparticles by physical adsorption. Put the prepared solution into a centrifuge tube, place it on a shaker for adsorption and fixation for 12 hours, centrifuge, wash with deionized water, and freeze-dry for use. Obtain enzyme-MHCS carbon spheres.

[0059] Example 4

[0060] The operations of steps (1) and (2) are the same as those of steps (1) and (2) of Example 1.

[0061] (3) Preparation of Zr-La-MHCS

[0062] 25 mg of lanthanum chloride (LaCl3), 25 mg of zirconium oxychloride octahydrate (ZrOCl2·8H2O) and 30 mg of the enzyme-linked carbon spheres prepared in step (2) were dispersed in 30 mL of HCl (0.1 M) solution, and stirred with a magnetic bar for 2.5 h at room temperature to chelate the metal ions with the enzyme. 14 mL of NaOH (1 M) solution was added to the solution in step 1, and the stirring reaction was continued for 2.5 h. The product was washed with deionized water and collected by centrifugation, and freeze-dried to obtain a double metal oxide functionalized double-layer mesoporous composite adsorbent (Zr-La-MHCS).

[0063] Example 5

[0064] The operations of steps (1) and (2) are the same as those of steps (1) and (2) of Example 1.

[0065] (3) Preparation of Zr-La-MHCS

[0066] 30 mg of lanthanum chloride (LaCl3), 30 mg of zirconium oxychloride octahydrate (ZrOCl2·8H2O) and 30 mg of the enzyme-linked carbon spheres prepared in step (2) were dispersed in 30 mL of HCl (0.1 M) solution, and stirred with a magnetic bar for 2.5 h at room temperature to chelate the metal ions with the enzyme. 14 mL of NaOH (1 M) solution was added to the solution in step 1, and the stirring reaction was continued for 2.5 h. The product was washed with deionized water and collected by centrifugation, and freeze-dried to obtain a double metal oxide functionalized double-layer mesoporous composite adsorbent (Zr-La-MHCS).

[0067] Example 6

[0068] The operations of steps (1) and (2) are the same as those of steps (1) and (2) of Example 1.

[0069] (3) Preparation of Zr-La-MHCS

[0070] 50 mg of lanthanum chloride (LaCl3), 50 mg of zirconium oxychloride octahydrate (ZrOCl2·8H2O) and 20 mg of the enzyme-linked carbon sphere prepared in step (2) were dispersed in 30 mL of HCl (0.1 M) solution, and stirred with a magnetic bar for 6 h at room temperature to chelate the metal ions with the enzyme. 14 mL of NaOH (1 M) solution was added to the solution in step 1, and the stirring reaction was continued for 6 h. The product was washed with deionized water and collected by centrifugation, and freeze-dried to obtain a double metal oxide functionalized double-layer mesoporous composite adsorbent (Zr-La-MHCS).

[0071] Comparative Example

[0072] Preparation of single-layer S-Zr-La-MHCS:

[0073] (1) Preparation of S-MHCS particles by polymerization

[0074] Tetrapropyl orthosilicate (TPOS, 3.46 mL), resorcinol (0.4 g) and formalin (37 wt%, 0.56 mL) were added to a solution consisting of aqueous ammonia solution (3.0 mL, 28 wt%), deionized water (10 mL) and ethanol (70 mL). The mixture was vigorously stirred at room temperature for 24 hours. The solid product was collected by centrifugation and dried overnight at 50 ° C. After carbonization at 70 ° C. N2 atmosphere and etching by hydrofluoric acid (HF, 5%) to remove the silica template, S-MHCS was obtained.

[0075] The operations of steps (2) and (3) are the same as those of steps (2) and (3) of Example 1 to obtain a single-layer S-Zr-La-MHCS.

[0076] The product Zr-La-MHCS obtained in Example 1 was subjected to performance testing:

[0077] like Figure 3 As shown, the adsorption solutions with pH values ​​ranging from 2-8 were studied and the corresponding zeta potential values ​​were determined. Because different pH values ​​will affect the zeta potential of the adsorbent surface, and also have a certain effect on the existence form of fluoride ions. When the zeta potential is high, the material has a higher adsorption capacity for fluoride ions, but when the pH is low, fluoride ions exist mainly in the form of HF, and the electrostatic effect is small at this time, so the adsorption capacity decreases. However, it still has a high adsorption capacity at other pH values, which means that the electrostatic effect of the double metal hydroxide grown on the surface of MHCS plays a major role in the adsorption of fluoride.

[0078] like Figure 4 As shown, the adsorption capacity of Zr-La-MHCS at different time nodes was investigated, and then the pseudo-first-order and pseudo-second-order kinetic models were used to fit the data, and the kinetics and fitting curves were drawn. The adsorption process of Zr-La-MHCS can be divided into three steps. It can be seen from the figure that the adsorption rate of fluoride ions in the material is relatively fast. In the first 10 minutes, through the electrostatic effect on the surface of the adsorbent, it began to adsorb rapidly, and the adsorption amount increased sharply. At 10min-30min, the adsorption rate decreased, and equilibrium was reached after about 50min. The adsorbent particles formed a strong complex with the fluoride ions. At the same time, the adsorption kinetics of different adsorbents under the same conditions were compared. The adsorption equilibrium time of the comparative example S-Zr-La-MHCS was similar to that of Zr-La-MHCS, but the adsorption equilibrium capacity was lower than that of Zr-La-MHCS, indicating that the adsorption capacity performance of the double-layer structure matrix material is higher. It can be seen from the figure that Zr-La-MHCS has a faster adsorption rate than commercial alumina adsorbents and a higher adsorption equilibrium capacity. In addition to the comparative tests of different adsorbents, the adsorption performance of Zr-La-MHCS adsorbent material at different volumes of fluorine solution was also studied. The adsorption equilibrium capacity was lower when the volume of fluorine solution was 20 mL, indicating that the adsorption performance was better when the feed ratio was 2 mg:9 mL.

[0079] Figure 5 The results of thermodynamic and adsorption model fitting curves were performed at 288K, 298K and 308K respectively. The adsorption capacity of Zr-La-MHCS increased with the increase of fluoride ion concentration, and the adsorption process was an endothermic process.

[0080] Figure 6 The effect of the concentration of competing ions on the adsorption and removal of fluorine by Zr-La-MHCS is shown. The initial concentration of fluorine ions was fixed at 20 mg L -1, the four interfering ions were prepared into mixed ion solutions at 0, 1, 2, and 5 times the concentration of fluoride ions, respectively. At room temperature, 2 mg of adsorbent and 9 mL of mixed ion solution were used for adsorption for 3 hours. After that, the fluoride ion concentration was determined by ion chromatography, and the adsorption capacity was calculated. When the concentration of nitrate ions changed, the degree of decrease in the adsorbent fluoride ion adsorption capacity was the smallest, and the concentration change of bicarbonate had a greater effect on the fluoride ion adsorption capacity, which may be because the hydrolysis of bicarbonate in water caused the pH to change and thus affected the adsorption process.

[0081] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a double-layer mesoporous composite adsorbent functionalized with a double metal oxide, characterized in that: The steps include: (1) Preparation of double-layer mesoporous hollow carbon spheres MHCS: Tetraethyl orthosilicate (TEOS), resorcinol and formalin were added to a solution consisting of an aqueous ammonia solution, deionized water and ethanol, and stirred vigorously at room temperature for t1, then TEOS was added and stirred for t2; finally, the solution was placed in a polytetrafluoroethylene-lined autoclave for further hydrothermal treatment, and the solid product was collected by centrifugation and dried overnight, and MHCS nanoparticles were obtained after carbonization under a N2 atmosphere and removal of the silica template by hydrofluoric acid etching; (2) Preparation of enzyme-MHCS: Take lysozyme LYM and add it to deionized water to prepare a lysozyme solution, add the MHCS nanoparticles prepared in step (1) to the lysozyme solution, and fix LYM on the MHCS nanoparticles by physical adsorption; then put the mixed solution into a centrifuge tube, place it on a shaker for adsorption and fixation, centrifuge, wash with deionized water, and freeze-dry for use, to obtain enzyme-MHCS carbon spheres; (3) Preparation of double-layer mesoporous composite adsorbent Zr-La-MHCS functionalized with double metal oxides: Lanthanum chloride LaCl3, zirconium oxychloride octahydrate ZrOCl2·8H2O and enzyme-MHCS were dispersed in HCl solution and stirred with a magnetic bar for a period of time to chelate the metal ions with the enzyme; then NaOH solution was added, the reaction was continued with stirring, centrifuged, washed with deionized water, and freeze-dried to obtain a double-metal oxide functionalized double-layer mesoporous composite adsorbent Zr-La-MHCS.

2. The preparation method according to claim 1, characterized in that In step (1), the amount ratio of tetraethyl orthosilicate TEOS, resorcinol, formalin, ammonia solution, deionized water, ethanol and TEOS is 2.8mL:0.4g:0.56mL:3.0mL:10mL:70mL:1.5mL; wherein the concentration of formalin is 37wt% and the concentration of ammonia solution is 28wt%; The stirring time t1 is 6 hours, and the stirring time t2 is 24 hours; The temperature of the hydrothermal treatment was 100°C and the time was 24 hours; The carbonization temperature was 700°C and the concentration of hydrofluoric acid was 5%.

3. The preparation method according to claim 1, characterized in that: In step (2), the usage ratio of lysozyme LYM and deionized water is 30-60 mg:30-50 mL; the mass volume ratio of MHCS and lysozyme aqueous solution is 30-60 mg:30-50 mL.

4. The preparation method according to claim 3, characterized in that: In step (2), the usage ratio of LYM and deionized water is 30 mg:40 mL; the mass volume ratio of MHCS and lysozyme aqueous solution is 20.0 mg:40 mL.

5. The preparation method according to claim 1, characterized in that: In step (2), the adsorption fixation time is 12.0 h.

6. The preparation method according to claim 1, characterized in that: In step (3), the mass volume ratio of LaCl3, ZrOCl2·8H2O, enzyme-MHCS and HCl solution is 20-50 mg: 20-50 mg: 20-50 mg: 20-50 mL.

7. The preparation method according to claim 6, characterized in that: In step (3), the mass volume ratio of LaCl3, ZrOCl2·8H2O, enzyme-MHCS and HCl solution is 25 mg:25 mg:50 mg:30 mL, wherein the concentration of HCl solution is 0.1 M.

8. The preparation method according to claim 1, characterized in that: In step (3), the volume ratio of NaOH solution to HCl solution is 10-20 mL:20-50 mL, wherein the concentration of NaOH solution is 1 M.

9. The preparation method according to claim 1, characterized in that: In step (3), the stirring reaction time is 2.5 hours at room temperature.

10. Use of the bimetallic oxide functionalized double-layer mesoporous composite adsorbent Zr-La-MHCS prepared by the preparation method according to any one of claims 1 to 9 for adsorption and separation of fluoride ions.

Citation Information

Patent Citations

  • Bio-adsorbent prepared by modifying ball-milled tea residues and preparation method and application of bio-adsorbent

    CN105688865A

  • Magnetic nano adsorbent for adsorbing mercury ions and preparation and application thereof

    CN110142031A

  • Method for preparing graphene cellulose aerogel loaded with lanthanum and zirconium bimetals

    CN110283361A

  • Functionalized silicon dioxide modified defluorination material as well as preparation and application thereof

    CN112777672A

  • Mixed metal oxide-hydroxide biopolymer composite beads and a process thereof

    US20230415121A1