Hydrodechlorination catalyst and preparation method thereof

Through alloy effect regulation of precious metals and organic phosphine ligands, a high-efficiency hydrodechlorination catalyst was prepared, which solved the problems of large equipment, low efficiency and insufficient catalyst activity selectivity in CTFE production, and achieved high conversion and high selectivity CTFE Production reduces production costs.

CN118892827APending Publication Date: 2024-11-05XIAN MODERN CHEM RES INST
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410918422.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing reduction and dechlorination method of 1,1,2-trifluoro-1,2,2-trichloroethane zinc powder has huge equipment, low production efficiency, high solvent consumption, and by-product zinc chloride treatment in CTFE production. Difficulties and other problems, and the catalytic activity and selectivity of the hydrodechlorination catalyst do not meet industrial requirements.

Method used

Using precious metals (Pd or Pt) as active components, combining metal additives and organic phosphine ligands, regulate electronic properties through alloying and coordination effects, prepare hydrodechlorination catalysts with high activity and stability, and pass wet The impregnation, calcination and reduction treatment process carried the medium onto activated carbon to form an efficient catalyst.

Benefits of technology

The high conversion rate of CFC-113 and the high selectivity of CTFE are achieved, which reduces production costs and is suitable for large-scale industrial production. The catalyst shows good activity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004935871260000031
    Figure BDA0004935871260000031
  • Figure BDA0004935871260000041
    Figure BDA0004935871260000041
  • Figure BDA0004935871260000071
    Figure BDA0004935871260000071
Patent Text Reader

Abstract

The invention discloses a hydrodechlorination catalyst and a preparation method thereof, the hydrodechlorination catalyst comprises active components, a metal additive, an organic phosphine ligand and an active carbon carrier, the active components are noble metals Pd and Pt, and the metal additive is selected from at least one of Ni, Cu, Ag and Ce. The hydrodechlorination catalyst has the advantages that the noble metal is used as an active component, and the electronic property of the noble metal is regulated and the noble metal nanoparticles are stabilized by utilizing the alloy effect and coordination effect of the metal additive and the organic phosphine ligand, so that the selectivity of the product is improved, and the service life of the catalyst is prolonged. The catalyst disclosed by the invention shows good activity and stability in the process of preparing chlorotrifluoroethylene through hydrodechlorination of 1, 1, 2-trifluoro-1, 2, 2-trichloroethane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a hydrodechlorination catalyst and a preparation method thereof, and belongs to the technical field of catalyst preparation for preparing chlorotrifluoroethylene by hydrodechlorination of 1,1,2-trifluoro-1,2,2-trichloroethane. Background Art

[0002] Chlorotrifluoroethylene (CTFE) is an important fluorine-containing monomer, and its usage is second only to tetrafluoroethylene and vinylidene fluoride. CTFE homopolymerization or copolymerization with other fluorine-containing monomers can be used to prepare polymer materials such as fluororesins, fluorine coatings, fluororubbers and chlorofluoro lubricants. These materials have good chemical stability, corrosion resistance, weather resistance, flame retardancy and dielectric properties. Therefore, they are widely used in high-tech fields such as national defense, aerospace, electronics industry, photovoltaic power generation, etc. In addition, CTFE is also an important fluorine-containing intermediate, which is used to synthesize downstream products such as trifluoroethylene, trifluorobromoethylene, hexafluorobutadiene and trifluorostyrene. As an intermediate product in the fluorine chemical industry chain, CTFE has a high added value and is an indispensable key material for strategic emerging industries. Therefore, the synthesis and production of CTFE have important practical significance.

[0003] At present, the production process of CTFE is the 1,1,2-trifluoro-1,2,2-trichloroethane (CFC-113) zinc powder reduction dechlorination method, which was first reported by Edward G.Locke et al. in 1934 and industrialized by EA Belmore et al. in 1947. The CFC-113 zinc powder reduction dechlorination method uses metal Zn powder as a reducing agent and methanol or ethanol as a reaction medium. The main products include CTFE and ZnCl2. This process route has the advantages of mild reaction conditions (80-110°C, 0.6-1.2MPa), mature production process and simple operation, but it also has the following problems: large production equipment, intermittent kettle operation, low production efficiency; the amount of Zn powder used is 1.3-1.5 times the theoretical amount, consuming a large amount of methanol or ethanol solvents and difficult to recover, and high production costs; a large amount of zinc chloride residue is produced as a by-product, which makes it difficult to treat the three wastes.

[0004] In response to the many problems of the Zn powder reduction dechlorination method, relevant scholars have proposed a new process route for preparing CTFE by gas-solid phase catalytic hydrodechlorination of CFC-113. This process is to replace Zn powder with H2 to react with CFC-113 under gas-solid phase catalytic conditions, and remove Cl atoms in the form of HCl molecules through hydrodechlorination reaction. Therefore, CFC-113 gas-solid phase catalytic hydrodechlorination has the advantages of being green, environmentally friendly, and can be produced continuously. In the process route of preparing CTFE by gas-solid phase catalytic hydrodechlorination of CFC-113, the catalyst is its technical core. According to existing literature reports, hydrodechlorination catalysts are mainly transition metal catalysts such as Ni and Co and precious metal catalysts such as Pd, Pt, and Ru, but their catalytic activity, trifluorochloroethylene selectivity, and catalyst stability still do not meet the requirements of industrial application.

[0005] European patent EP0053657B1 discloses a hydrodechlorination catalyst, wherein a platinum metal is loaded onto a basic magnesium fluoride (such as sodium magnesium fluoride, potassium magnesium fluoride) carrier to obtain a catalyst, and then the catalyst is used in the process of preparing trifluorochloroethylene by hydrodechlorination of CFC-113. Before the reaction, the catalyst is treated with hydrogen reduction activation at a temperature of 400 to 600°C to reduce all active components to a metallic state. The CFC-113 conversion rate of the reported catalyst is less than 50%, and the conversion rate and selectivity of the catalyst have a "seesaw" effect, and it is impossible to simultaneously meet high conversion rate and high selectivity. Summary of the invention

[0006] The present invention provides a hydrodechlorination catalyst and a preparation method thereof, wherein a noble metal is used as an active component, and the alloy effect and coordination effect of a metal additive and an organic phosphine ligand are used to regulate the electronic properties of the noble metal and stabilize the noble metal nanoparticles, thereby improving the selectivity of the product and the service life of the catalyst. The catalyst disclosed in the present invention exhibits good activity and stability in the process of preparing chlorotrifluoroethylene by hydrodechlorination of 1,1,2-trifluoro-1,2,2-trichloroethane.

[0007] To achieve the above object, the technical solution adopted by the present invention includes:

[0008] A hydrodechlorination catalyst comprises a carrier, wherein the carrier carries an active component, a metal promoter and an organic phosphorus ligand; in terms of mass percentage of the total amount of the catalyst:

[0009] The active component is Pd or Pt, with a mass fraction of 0.05% to 2%;

[0010] The metal additive is selected from at least one of Ni, Cu, Ag and Ce, with a mass fraction of 0.1% to 40%;

[0011] The organic phosphine ligand is selected from at least one of dimethylphosphonic acid, n-hexylphosphonic acid, n-heptylphosphonic acid, n-octylphosphonic acid, n-nonylphosphonic acid, n-decylphosphonic acid, dodecylphosphonic acid, tetradecylphosphonic acid, 1,4-butanediphosphonic acid, vinylphosphonic acid, phenylphosphonic acid, benzylphosphonic acid and phenylethylphosphonic acid, and the mass fraction is 1% to 40%.

[0012] Optionally, the mass fraction of the active component is 0.5-1.5%; the mass fraction of the metal additive is 5-10%; and the mass fraction of the organic phosphine ligand is 10-20%.

[0013] Optionally, the mass fraction of the active component is 1%.

[0014] Optionally, the mass fraction of the metal additive is 7.5%.

[0015] Optionally, the mass fraction of the organic phosphine ligand is 15%.

[0016] Preferably, the mass fraction of the active component is 0.05%; the mass fraction of the metal auxiliary agent is 0.1%; and the mass fraction of the organic phosphine ligand is 1%.

[0017] Preferably, the mass fraction of the active component is 0.5%; the mass fraction of the metal auxiliary agent is 5%; and the mass fraction of the organic phosphine ligand is 20%.

[0018] Preferably, the mass fraction of the active component is 2%; the mass fraction of the metal auxiliary agent is 40%; and the mass fraction of the organic phosphine ligand is 40%.

[0019] Preferably, the mass fraction of the active component is 0.5%; the mass fraction of the metal auxiliary agent is 5%; and the mass fraction of the organic phosphine ligand is 10%.

[0020] Preferably, the mass fraction of the active component is 1%; the mass fraction of the metal auxiliary agent is 10%; and the mass fraction of the organic phosphine ligand is 20%.

[0021] Optionally, the carrier is activated carbon, and the specific surface area of ​​the activated carbon carrier is greater than 700m 2 / g, micropore volume is greater than 0.35cm 3 / g, pH value is less than 5.0.

[0022] The method for preparing any of the hydrodechlorination catalysts of the present invention comprises:

[0023] The active component, the metal auxiliary agent and the organic phosphine ligand are loaded onto the carrier by a wet impregnation method, and the hydrodechlorination catalyst can be obtained by sequentially performing drying, calcination treatment and reduction treatment.

[0024] Optionally, the wet impregnation comprises: immersing the carrier in a mixed solution of active components, metal additives and organic phosphine ligands at 20° C. to 80° C. for 8 h to 24 h.

[0025] Optionally, the calcination treatment is carried out in a nitrogen atmosphere at a calcination temperature of 160°C to 400°C.

[0026] Optionally, the reduction treatment is carried out in a hydrogen atmosphere at a reduction temperature of 160°C to 320°C.

[0027] The beneficial effects of the present invention include:

[0028] The hydrodechlorination catalyst provided in the present application has the advantages of simple preparation process, low production cost, mild reaction conditions, excellent catalytic performance, and suitability for large-scale industrial production. -1 Under the conditions of , the conversion rate of CFC-113 reached over 96.5% and the selectivity of CTFE reached over 94.8%. DETAILED DESCRIPTION

[0029] The present application is described in detail below in conjunction with the examples, but the present application is not limited to these examples. Unless otherwise specified, the raw materials in the examples of the present application are purchased through commercial channels.

[0030] The abbreviations of the relevant chemical substances in this application are as follows:

[0031] Dimethylphosphonic acid (DMPA), n-hexylphosphonic acid (HPA), n-heptylphosphonic acid (HTPA), n-octylphosphonic acid (OPA), n-nonylphosphonic acid (NPA), n-decylphosphonic acid (DEPA), dodecylphosphonic acid (DODEPA), tetradecylphosphonic acid (TEDEPA), 1,4-butanediphosphonic acid (BDPA), vinylphosphonic acid (VPA), phenylphosphonic acid (BPA), benzylphosphonic acid (PMPA), phenylethylphosphonic acid (PEPA).

[0032] In the examples of this application, the conversion rate and selectivity are calculated as follows:

[0033]

[0034]

[0035] In this application, gas chromatography is used to analyze the composition of the product at the outlet of the reactor. The model of the gas chromatograph is Agilent Technologies 7890B, the chromatographic detector is an FID detector, and the model of the chromatographic column is Gas-Pro. In chromatographic analysis, the peak area of ​​the chromatographic peak is proportional to the concentration of the component to be tested; in the chromatographic column, the sample to be tested is separated into individual components, and flows out of the chromatographic column in a certain order, enters the detector, and is converted into an electrical signal, which is then amplified and recorded by a recorder, and a set of curves are obtained on the recording paper. According to the peak area of ​​the chromatographic peak, the content of each component in the sample can be quantitatively determined, and then the CFC-113 conversion rate and CTFE selectivity can be calculated.

[0036] In a first aspect of the present application, a hydrodechlorination catalyst is provided, which comprises an active component, a metal promoter, an organic phosphine ligand and an activated carbon carrier, wherein the active component, the metal promoter and the organic phosphine ligand are loaded on the activated carbon carrier.

[0037] The active component is precious metal Pd or Pt, and the mass fraction of the precious metal in the catalyst is 0.05% to 2%.

[0038] The metal additive is selected from at least one of Ni, Cu, Ag and Ce, and the mass fraction of the metal additive is 0.1% to 40%.

[0039] The mass fraction of the organic phosphine ligand in the catalyst is 1% to 40%, and the organic phosphine ligand is an alkyl phosphonic acid; the alkyl phosphonic acid is selected from at least one of dimethyl phosphonic acid, n-hexyl phosphonic acid, n-heptyl phosphonic acid, n-octyl phosphonic acid, n-nonyl phosphonic acid, n-decyl phosphonic acid, dodecyl phosphonic acid, tetradecyl phosphonic acid, 1,4-butanediphosphonic acid, vinyl phosphoric acid, phenyl phosphonic acid, benzyl phosphonic acid and phenylethyl phosphonic acid.

[0040] The specific surface area of ​​the activated carbon carrier is greater than 700m 2 / g, micropore volume is greater than 0.35cm 3 / g, pH value is less than 5.0.

[0041] According to another aspect of the present application, a method for preparing any of the above hydrodechlorination catalysts is also provided, wherein the active component, metal additive and organic phosphine ligand are loaded onto the activated carbon carrier by a wet impregnation method to obtain the hydrodechlorination catalyst.

[0042] The wet impregnation method includes at least one of equal volume impregnation and excess impregnation.

[0043] During the equal volume impregnation process, the mass ratio of the catalyst support to the mass ratio of the mixed solution of the active component, the metal promoter and the organic phosphine ligand is 0.6 to 1.2.

[0044] In the solution of the active component, the solvent may be deionized water, ethanol or a mixed solution of ethanol and water.

[0045] Equal volume impregnation or excess impregnation is carried out under closed conditions.

[0046] The preparation method of the hydrodechlorination catalyst comprises at least the following steps:

[0047] (A) Immerse the catalyst support in a mixed solution of active components, metal additives and organic phosphine ligands at 20° C. to 80° C. for 8 h to 24 h.

[0048] Specifically, in step (A), the temperature of equal volume impregnation or excess impregnation is selected from any value among 20°C, 40°C, 60°C and 80°C or any range between two values.

[0049] Specifically, in step (A), the time for equal volume impregnation or excess impregnation is selected from any value among 8 h, 12 h, 16 h, 20 h and 24 h, or any range between two of them.

[0050] (B) The impregnated catalyst is placed in a vacuum drying oven and dried at 80-120° C. for 8-12 hours.

[0051] Specifically, in step (B), the drying temperature is selected from any value among 80°C, 90°C, 100°C, 110°C and 120°C, or any range between two values.

[0052] (C) The dried catalyst was placed in a tubular furnace and calcined at 160-400° C. for 4 h in a nitrogen atmosphere.

[0053] Specifically, in step (C), the calcination temperature is selected from any value of 160°C, 200°C, 240°C, 280°C, 320°C, 360°C and 400°C, or any range between two values.

[0054] (D) The calcined catalyst is placed in a tubular furnace and reduced in a hydrogen atmosphere at 160-320° C. for 2-8 hours.

[0055] Specifically, in step (D), the reduction temperature is selected from any value of 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C and 320°C, or any range therebetween.

[0056] Specifically, in step (D), the reduction time is selected from any value among 2 h, 4 h, 6 h and 8 h, or any range value therebetween.

[0057] The hydrodechlorination catalyst is used in the process of preparing CTFE by hydrodechlorination of CFC-113. The raw gas containing CFC-113 and H2 is contacted with the hydrodechlorination catalyst to react and obtain CTFE.

[0058] The gas volume space velocity of the raw material is 30~1440h -1 ; The reaction temperature is 120-240°C; The ratio of H2 to CFC-113 in the raw gas is 1.0-10.0.

[0059] The reaction was carried out in a fixed bed reactor.

[0060] The raw gas volume space velocity is selected from 30h -1 , 120h -1 、360h -1 , 720h -1 , 1080h -1 and 1440h -1 Any value in between or any range of values ​​between them.

[0061] The reaction temperature is selected from any value among 120°C, 140°C, 160°C, 180°C, 200°C, 220°C and 240°C, or any range therebetween.

[0062] The molar ratio of H2 to CFC-113 is selected from any value among 1.0, 2.0, 4.0, 6.0, 8.0, 10.0 or any range between two values.

[0063] Example 1 Preparation of 0.05Pd-0.1Ag-1DMPA / AC Catalyst

[0064] First, 0.0083g PdCl2, 0.0158g AgNO3 and 0.1g DMPA were dissolved in 8.00g anhydrous ethanol, and stirred at 60°C for 5min to completely dissolve the solid mixture to obtain an impregnation solution; secondly, 10.00g pretreated activated carbon carrier was added to the above impregnation solution to make the impregnation solution completely absorbed by the activated carbon carrier, and the solid-liquid mixture was sealed and impregnated at 25°C for 12h to complete the impregnation process; then, it was calcined at 200°C in a nitrogen atmosphere for 4h, and the heating program was: 20°C-200°C, 5°C / min; finally, it was reduced at 240°C in a hydrogen atmosphere for 4h, and the heating program was: 20°C-240°C, 5°C / min, and cooled to room temperature to obtain 0.05Pd-0.1Ag-1DMPA / AC catalyst.

[0065] Example 2 Preparation of 0.5Pd-5Cu-20HPA / AC Catalyst

[0066] Firstly, 0.0833g PdCl2, 1.3424g CuCl2·2H2O and 1.00g HPA were dissolved in 8.00g anhydrous ethanol, and stirred at 60°C for 5min to completely dissolve the solid mixture to obtain an impregnation solution; secondly, 10.00g pretreated activated carbon carrier was added to the impregnation solution to make the impregnation solution completely absorbed by the activated carbon carrier, and the solid-liquid mixture was sealed and impregnated at 25°C for 12h to complete the impregnation process; then, it was calcined at 200°C in a nitrogen atmosphere for 4h, and the temperature program was: 20°C-200°C, 5°C / min; finally, it was reduced at 240°C in a hydrogen atmosphere for 4h, and the temperature program was: 20°C-240°C, 5°C / min, and cooled to room temperature to obtain 0.5Pd-5Cu-20HPA / AC catalyst.

[0067] Example 3 Preparation of 2Pd-40Cu-40OPA / AC Catalyst

[0068] Firstly, 0.3332g PdCl2, 5.3696g CuCl2·2H2O and 4.00g OPA were dissolved in 8.00g anhydrous ethanol, and stirred at 60°C for 5min to completely dissolve the solid mixture to obtain an impregnation solution; secondly, 10.00g pretreated activated carbon carrier was added to the impregnation solution to make the impregnation solution completely absorbed by the activated carbon carrier, and the solid-liquid mixture was sealed and impregnated at 25°C for 12h to complete the impregnation process; then, it was calcined at 200°C in a nitrogen atmosphere for 4h, and the temperature program was: 20°C-200°C, 5°C / min; finally, it was reduced at 240°C in a hydrogen atmosphere for 4h, and the temperature program was: 20°C-240°C, 5°C / min, and cooled to room temperature to obtain a 2Pd-40Cu-40OPA / AC catalyst.

[0069] Example 4 Preparation of 0.5Pt-5Ni-10DODEPA / AC Catalyst

[0070] Firstly, 0.1050g H2PtCl6, 2.0249g NiCl2·6H2O and 1.00g DODEPA were dissolved in 8.00g anhydrous ethanol, and stirred at 60°C for 5min to completely dissolve the solid mixture to obtain an impregnation solution; secondly, 10.00g pretreated activated carbon carrier was added to the above impregnation solution to make the impregnation solution completely absorbed by the activated carbon carrier, and the solid-liquid mixture was sealed and impregnated at 25°C for 12h to complete the impregnation process; then, it was calcined at 200°C in a nitrogen atmosphere for 4h, and the heating program was: 20°C-200°C, 5°C / min; finally, it was reduced at 240°C in a hydrogen atmosphere for 4h, and the heating program was: 20°C-240°C, 5°C / min, and cooled to room temperature to obtain 0.5Pt-5Ni-10DODEPA / AC catalyst.

[0071] Example 5 Preparation of 1Pt-10Ce-20BPA / AC Catalyst

[0072] First, 0.2100g H2PtCl6, 1.7590g CeCl3 and 2.00g BPA were dissolved in 8.00g anhydrous ethanol, and stirred at 60°C for 5min to completely dissolve the solid mixture to obtain an impregnation solution; secondly, 10.00g pretreated activated carbon carrier was added to the above impregnation solution to make the impregnation solution completely absorbed by the activated carbon carrier, and the solid-liquid mixture was sealed and impregnated at 25°C for 12h to complete the impregnation process; then, it was calcined at 200°C in a nitrogen atmosphere for 4h, and the heating program was: 20°C-200°C, 5°C / min; finally, it was reduced at 240°C in a hydrogen atmosphere for 4h, and the heating program was: 20°C-240°C, 5°C / min, and cooled to room temperature to obtain 1Pt-10Ce-20BPA / AC catalyst.

[0073] Example 6 Preparation of 1.5Pt-7.5Cu-15PMPA / AC Catalyst

[0074] Firstly, 0.3150g H2PtCl6, 2.0136g CuCl2·2H2O and 1.50g PMPA were dissolved in 8.00g anhydrous ethanol, and stirred at 60°C for 5min to completely dissolve the solid mixture to obtain an impregnation solution; secondly, 10.00g pretreated activated carbon carrier was added to the impregnation solution to make the impregnation solution completely absorbed by the activated carbon carrier, and the solid-liquid mixture was sealed and impregnated at 25°C for 12h to complete the impregnation process; then, it was calcined at 200°C in a nitrogen atmosphere for 4h, and the temperature program was: 20°C-200°C, 5°C / min; finally, it was reduced at 240°C in a hydrogen atmosphere for 4h, and the temperature program was: 20°C-240°C, 5°C / min, and cooled to room temperature to obtain a 1.5Pt-7.5Cu-15PMPA / AC catalyst.

[0075] Example 7 Catalyst Evaluation Experiment

[0076] The process of preparing CTFE by hydrodechlorination of CFC-113 was carried out in a fixed bed reactor. The reactor material was 316L alloy, the inner diameter of the reactor was 10 mm, the length was 450 mm, and 10 mL of the catalyst prepared in Examples 1 to 6 was loaded respectively. High-purity nitrogen was introduced before the reaction for drying and dehydration at elevated temperature, and then the raw gas volume space velocity was 30 h -1 ~1440h -1 The reaction temperature was 120°C to 240°C, the ratio of H2 to CFC-113 in the feed gas was 1.0 to 10.0, and the pressure in the reactor was 100 kPa. The products after the reaction were analyzed by gas chromatography. The results of conversion rate and selectivity are shown in Table 1.

[0077] Table 1 Catalyst evaluation results

[0078]

[0079] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A hydrodechlorination catalyst, characterized in that It comprises a carrier, on which active components, metal additives and organic phosphorus ligands are supported; Calculated by mass percentage of the total catalyst: The active component is Pd or Pt, with a mass fraction of 0.05% to 2%; The metal additive is selected from at least one of Ni, Cu, Ag and Ce, with a mass fraction of 0.1% to 40%; The organic phosphine ligand is selected from at least one of dimethylphosphonic acid, n-hexylphosphonic acid, n-heptylphosphonic acid, n-octylphosphonic acid, n-nonylphosphonic acid, n-decylphosphonic acid, dodecylphosphonic acid, tetradecylphosphonic acid, 1,4-butanediphosphonic acid, vinylphosphonic acid, phenylphosphonic acid, benzylphosphonic acid and phenylethylphosphonic acid, and the mass fraction is 1% to 40%.

2. The hydrodechlorination catalyst according to claim 1, characterized in that The mass fraction of the active component is 0.5-1.5%; the mass fraction of the metal auxiliary agent is 5-10%; and the mass fraction of the organic phosphine ligand is 10-20%.

3. The hydrodechlorination catalyst according to claim 1 or 2, characterized in that The mass fraction of the active component is 1%.

4. The hydrodechlorination catalyst according to claim 1 or 2, characterized in that The mass fraction of the metal additive is 7.5%.

5. The hydrodechlorination catalyst according to claim 1 or 2, characterized in that The mass fraction of the organic phosphine ligand is 15%.

6. The hydrodechlorination catalyst according to any one of claims 1 to 5, characterized in that The carrier is activated carbon, and the specific surface area of ​​the activated carbon carrier is greater than 700m 2 / g, micropore volume is greater than 0.35cm 3 / g, pH value is less than 5.

0.

7. The method for preparing the hydrodechlorination catalyst according to any one of claims 1 to 5, characterized in that: include: The active component, the metal auxiliary agent and the organic phosphine ligand are loaded onto the carrier by a wet impregnation method, and the hydrodechlorination catalyst can be obtained by sequentially performing drying, calcination treatment and reduction treatment.

8. The method for preparing a hydrodechlorination catalyst according to claim 7, characterized in that: The wet impregnation comprises: The carrier is immersed in a mixed solution of active components, metal additives and organic phosphine ligands at 20° C. to 80° C. for 8 h to 24 h.

9. The method for preparing a hydrodechlorination catalyst according to claim 7, characterized in that: The calcination treatment is carried out in a nitrogen atmosphere at a calcination temperature of 160°C to 400°C.

10. The method for preparing a hydrodechlorination catalyst according to claim 7, characterized in that: The reduction treatment is carried out in a hydrogen atmosphere at a reduction temperature of 160°C to 320°C.

Citation Information

Patent Citations

  • Preparation of chlorotrifluoroethylene and trifluoroethylene

    EP0053657B1

  • Hydrodechlorination catalyst and application thereof in preparation of chlorotrifluoroethylene

    CN105457651A

  • A catalyst for selective hydrodechlorination to prepare trifluorochloroethylene

    CN109967101A

  • Catalyst for preparing trifluorochloroethylene and trifluoroethylene by using CFC-113 catalytic hydro-dechlorination and its preparation method

    CN1460549A

  • Process for the preparation of trichloroethylene

    DE3804265A1