Monatomic iron catalyst for degrading organic pollutants by persulfate method as well as preparation and application of monatomic iron catalyst

Through the application of wool protein carbon-supported single-atom iron catalyst, the pH dependence and circulation rate limiting of the traditional iron ion activated persulfate method is solved, and efficient catalytic activation of persulfate is achieved, which improves the stability and recycling of the catalyst. It reduces the cost of wastewater treatment and promotes environmental protection.

CN118892832AActive Publication Date: 2024-11-05HEBEI XINDADONG TEXTILE CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410952342.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The advanced oxidation process of traditional iron ion activated persulfate method has problems such as pH dependence, Fe3+/Fe2+ cycle rate limit and inability to recycle, resulting in low catalytic activation efficiency and environmental pollution.

Method used

The single-atom iron catalyst with wool protein carbon supported by reducing pretreatment-formic acid method is used to dissolve wool protein, and the lipoic acid is modified to complex with iron ions to form a porous structure. It can activate persulfate acid under different pH environments. salt improves catalytic efficiency and realizes the recycling of catalysts.

Benefits of technology

It significantly improves the efficiency of catalytically activated persulfate, breaks the Fe3+/Fe2+ cycle rate limit, the catalyst has high activity, stability and low cost, can be recycled and used multiple times, reduces the cost of wastewater treatment, promotes green development and environmental protection. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892832A_ABST
    Figure CN118892832A_ABST
Patent Text Reader

Abstract

The invention discloses a monatomic iron catalyst for degrading organic pollutants by a persulfate method, the monatomic iron catalyst is a modified wool protein carbon-loaded asymmetric coordination monatomic iron catalyst, and the monatomic iron catalyst is prepared by modifying a wool protein solution dissolved by a reduction pretreatment-formic acid method with lipoic acid and then complexing with iron ions; and finally, freeze-drying, calcining at high temperature and pickling. The obtained monatomic iron catalyst has the advantages of high activity, high stability, low cost, simplicity in operation and the like, is applied to a reaction for catalytically activating persulfate to degrade organic pollutants, and can break through the Fe < 3 + > / Fe < 2 + > circulation rate limitation existing in the existing iron ion activation process, so that the monatomic iron catalyst shows excellent adsorption and catalysis efficiency and has a wide application prospect. And the activation process does not need pH environment limitation, the cycling stability is good, and the application of a persulfate-process advanced oxidation process in wastewater treatment is remarkably promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalysts, and in particular to a single-atom iron catalyst for degrading organic pollutants by a persulfate method, and the preparation and application of the catalyst. Background Art

[0002] Advanced oxidation processes (AOPs) are typical and effective methods for treating refractory organic matter in wastewater. They use the strong oxidizing free radicals generated by the reaction system to decompose organic pollutants in the water into small molecules, or even mineralize them into CO2, H2O and corresponding inorganic ions, to achieve the purpose of completely removing pollutants. Among them, the advanced oxidation process based on persulfate (i.e., persulfate-based advanced oxidation process PS-AOPs) has attracted more and more attention due to its high removal efficiency, simple operation and strong versatility. Persulfate ionizes in water to produce persulfate ions, and its standard redox potential E 0 The voltage reaches +2.01V. The molecule contains peroxide -OO-, which is a strong oxidant. However, persulfate is generally stable and has a low reaction rate. It can be activated into sulfate radicals under the conditions of transition metal ions (such as iron, silver, cobalt, etc.). Under the environment of pH>8.5, sulfate radicals oxidize water or OH. - Production of hydroxyl radicals, redox potential E 0 = +2.6V, which is much higher than persulfate ion and close to hydroxyl radical, with strong oxidizing ability and high pollutant removal efficiency. Since iron ions are widely present, cheap and easy to obtain, and less polluting, the activation efficiency of persulfate is also very high. Therefore, most of them use iron ions to activate the persulfate reaction system. However, the traditional iron ion activation process of persulfate has always faced pH dependence and the difficulty of breaking Fe 3+ / Fe 2+ Due to application bottlenecks such as cycle rate limitations and inability to recycle, the development of catalysts with high activity and high stability for catalytic activation of persulfate to enhance the degradation of organic pollutants is the research focus of this type of catalyst. Summary of the invention

[0003] In order to solve the application bottleneck of the prior art of using iron ions to activate persulfate for advanced oxidation process, the present invention provides a single-atom iron catalyst, which is used to catalyze the activation of persulfate to degrade organic pollutants, and can break the Fe 3+ / Fe 2+ The cycle rate is limited, showing excellent adsorption and catalytic efficiency, and the activation process does not require a pH environment, with good cycle stability, which significantly promotes the application of persulfate advanced oxidation process in wastewater treatment.

[0004] The single-atom iron catalyst for degrading organic pollutants by the persulfate method of the present invention is a wool protein carbon-loaded asymmetric coordinated single-atom iron catalyst, which is prepared by dissolving a wool protein solution by reduction pretreatment-formic acid method, modifying it with lipoic acid, and then complexing it with iron ions, and finally freeze-drying, high-temperature calcining, and acid washing.

[0005] Conventional use of transition metal ions to activate persulfate, because metal ion activation can cause the valence state of metal ions to change, so that the activity is reduced; and metal ions are difficult to recycle, which can cause water pollution. The single-atom iron catalyst of the present invention uses low-priced, long-life Fe as the catalytic active center, and utilizes thioctic acid to modify wool protein and then complex iron ions. Because thioctic acid and wool protein contain abundant nitrogen and sulfur, sufficient anchoring sites can be provided for iron ions and prevent their aggregation and migration. Finally, sulfur and nitrogen anchored carbon-loaded single-atom iron in a porous structure is formed by high-temperature calcination. The porous structure can increase the specific surface area, fully contact with persulfate, and greatly improve the catalytic efficiency. At the same time, relative to iron ions, the single-atom iron catalyst is used because the anchoring of iron atoms by the supporting material, and the iron atoms will not be leached into the solution, and can be recycled many times without forming iron element pollution to the environment.

[0006] The wool protein solution was prepared using the "reduction pretreatment-formic acid" dissolution method. First, the disulfide bonds in the wool were reduced using tri(2-carboxyethyl)phosphine hydrochloride solution, which has a highly selective reduction of disulfide bonds, to make the wool protein soluble in water. Then, the wool protein was grafted with lipoic acid to change the molecular structure and aggregation form of the polypeptide, making it easier for the molecules to form parallel or folded arrangements, providing sufficient sulfur anchoring sites for iron ions. Most of the formic acid reagent in the wool protein was then removed by dialysis, allowing the iron ions to combine with the modified wool protein by Coulomb force. Finally, the protein gel was obtained by freeze-drying, and the iron ions were reduced to the atomic level by high-temperature calcination and acid washing to obtain a single-atom iron catalyst.

[0007] As a limitation of the above technical solution, the wool protein solution is prepared by adding wool to a tri(2-carboxyethyl)phosphine hydrochloride solution, treating the wool at 70-90° C., and then adding the treated wool fibers to formic acid to fully dissolve the wool fibers.

[0008] As a limitation of the above technical solution, the wool protein complexed with lipoic acid modified with iron ions is prepared by adding lipoic acid powder to a wool protein solution, stirring the reaction at 30-50°C, then dialyzing the solution, adding an iron precursor, and stirring the mixture sufficiently at 30-40°C.

[0009] As a limitation of the above technical solution, the amount of wool is 1-2 g, the concentration of tri(2-carboxyethyl)phosphine hydrochloride solution is 80-120 g / L, the amount is 10-50 mL, the amount of formic acid is 20-50 mL, the amount of lipoic acid is 0.5-10 g, and the amount of iron precursor is 0.1-0.2 g.

[0010] As a limitation of the above technical solution, the iron precursor is selected from at least one of ferric acetylacetonate, ferric chloride, ferrous chloride, ferrous nitrate, ferric sulfate and ferrous sulfate.

[0011] As a limitation of the above technical solution, the freeze-drying temperature is -40 to -60°C; the high-temperature calcination temperature is 700 to 1000°C; and the acid washing uses HCl solution.

[0012] Further limiting the preparation conditions of the catalyst, such as the reaction treatment conditions, the amount of raw materials, etc., effectively regulates the microstructure of the catalyst, especially the size and electronic structure of the active center Fe, to achieve effective control of the substrate reaction kinetics, thereby obtaining a high catalytic rate for the activated persulfate reaction.

[0013] The present invention also provides the preparation of the single-atom iron catalyst for degrading organic pollutants by the persulfate method as described above, comprising the following preparation steps:

[0014] a. Add 1-2 g of wool to 10-50 mL of 80-120 g / L tris(2-carboxyethyl)phosphine hydrochloride solution, treat at 70-90° C. for 1-3 h to obtain wool fiber, add the wool fiber to 20-50 mL of formic acid, stir at 50-70° C. for 4-6 h to fully dissolve, centrifuge, and obtain the supernatant as the wool protein solution;

[0015] b. Add 0.5-10 g of lipoic acid powder to the wool protein solution, stir and react at 30-50° C. for 1-3 h to obtain a modified wool protein solution, put it into a dialysis bag, and perform dialysis with deionized water;

[0016] c. Add 0.1-0.2 g of iron precursor to the dialyzed modified wool protein solution, stir at 30-40° C. for 1-6 h, and freeze-dry the resulting solution at -40--60° C. for 12-48 h to obtain a protein gel;

[0017] d. Calcine the protein gel at 700-1000° C. for 1-4 h, and then wash the calcined product with HCl solution, wash with water, and dry to obtain a single-atom iron catalyst.

[0018] As a limitation of the above technical solution, in step a, the centrifugal speed is 10000 r / min and the time is 5 min; and / or;

[0019] In step b, the dialysis treatment is performed by replacing deionized water every 30 to 40 minutes for 3 to 4 hours; and / or;

[0020] In step d, the calcination temperature is 800-900° C. and the time is 1-3 hours; and / or;

[0021] The calcined product is acid-washed in a 0.2-0.6 mol / L HCl solution for 12-24 h, then washed with deionized water and dried.

[0022] Improve the preparation of single-atom iron catalysts to significantly improve catalytic activity and applicability in advanced oxidation processes.

[0023] At the same time, the present invention further provides the use of the single-atom iron catalyst for degrading organic pollutants by the persulfate method as described above, and the single-atom iron catalyst is used as a catalyst for activating persulfate to replace the soluble iron salt catalyst used in the persulfate advanced oxidation process.

[0024] As a limitation of the above technical solution, the single-atom iron catalyst is suitable for acidic or alkaline reaction systems, and can be recovered and repeatedly used in persulfate advanced oxidation processes.

[0025] The single-atom iron catalyst of the present invention can activate persulfate under normal temperature and pressure and pH-independent reaction environment, thereby degrading macromolecular organic matter in industrial wastewater, and degrading toxic macromolecular organic matter into non-toxic or low-toxic small molecular substances. The catalyst not only has high catalytic efficiency and activity, but also has good stability and can be recycled and reused, greatly reducing the cost of wastewater treatment, promoting green development, and protecting the environment and human health. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 , is a spherical aberration electron microscope image of the single-atom iron catalyst obtained in Example 1 of the present invention;

[0027] Figure 2 , is a scanning electron microscope image of the single-atom iron catalyst obtained in Example 1 of the present invention;

[0028] Figure 3 , is the EXAFS spectrum of the single-atom iron catalyst obtained in Example 1 of the present invention;

[0029] Figure 4 , is the XANES spectrum of the single-atom iron catalyst obtained in Example 1 of the present invention;

[0030] Figure 5 , is a gas chromatogram of the initial solution of p-chlorophenol in Example 1 of the present invention;

[0031] Figure 6, is the gas chromatogram of the solution after para-chlorophenol is degraded for 30 minutes in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The raw materials involved in the following examples and comparative examples are typical products purchased from the market.

[0034] Example 1

[0035] An iron atom catalyst, the preparation operation of which is carried out according to the following steps:

[0036] a. Weigh 1g of wool and add it to 10mL of 120g / L tri(2-carboxyethyl)phosphine hydrochloride solution, treat it at 70℃ for 2h, add the treated wool fiber to 30mL of formic acid, stir it at 70℃ for 6h to fully dissolve it, centrifuge it at 10000r / min for 5min, and the supernatant obtained is the wool protein solution;

[0037] b. Add 5 g of lipoic acid powder to the wool protein solution obtained in step a, stir and react at 50° C. for 2 h to obtain a modified wool protein solution, then put it into a dialysis bag, and perform dialysis with deionized water as the dialysis fluid. Change the deionized water every 30 min, and continue dialysis for 4 h;

[0038] c. Add 0.15 g of Fe(NO3)3·9H2O to the modified wool protein solution after dialyzation in step b, stir at 40°C for 4 h, and freeze-dry the resulting solution at -40°C for 12 h to obtain a protein gel;

[0039] d. Calcine the protein gel at 900° C. in a tube furnace for 2 h, then acid-wash it in a 0.3 mol / L HCl solution for 12 h, then wash it with deionized water and dry it to obtain a single-atom iron catalyst.

[0040] The structure of the obtained single-atom iron catalyst was analyzed. Figure 1 Spherical aberration electron microscope image, Figure 2 Scanning electron micrographs of Figure 3 The EXAFS spectrum of Figure 4From the XANES spectrum, it can be seen through spherical aberration electron microscopy that Fe is an isolated single atom. Using scanning electron microscopy, it can be seen that the catalyst as a whole has a porous structure. With the help of synchrotron radiation analysis, it can be seen that the catalyst has rich sulfur coordination, forming a Fe1S1N3 structure.

[0041] Example 2

[0042] An iron atom catalyst, the preparation operation of which is carried out according to the following steps:

[0043] a. Weigh 1g of wool and add it to 20mL of 120g / L tri(2-carboxyethyl)phosphine hydrochloride solution, treat it at 80℃ for 2h, add the treated wool fiber to 30mL of formic acid, stir it at 60℃ for 6h to fully dissolve it, centrifuge it at 10000r / min for 5min, and the supernatant obtained is the wool protein solution;

[0044] b. Add 3 g of lipoic acid powder to the wool protein solution obtained in step a, stir and react at 50° C. for 2 h to obtain a modified wool protein solution, then put it into a dialysis bag, and perform dialysis with deionized water as the dialysis fluid. Change the deionized water every 40 min, and continue dialysis for 4 h;

[0045] c. Add 0.15 g of Fe(NO3)3·9H2O to the modified wool protein solution after dialyzation in step b, stir at 40°C for 4 hours, and freeze-dry the solution at -40°C for 18 hours to obtain a protein gel;

[0046] d. Calcine the protein gel at 800° C. in a tube furnace for 2 h, then acid-wash it in a 0.3 mol / L HCl solution for 24 h, then wash it with deionized water and dry it to obtain a single-atom iron catalyst.

[0047] Example 3

[0048] An iron atom catalyst, the preparation operation of which is carried out according to the following steps:

[0049] a. Weigh 1.5g of wool and add it to 20mL of 100g / L tri(2-carboxyethyl)phosphine hydrochloride solution, treat it at 70℃ for 2h, add the treated wool fiber to 50mL of formic acid, stir it at 70℃ for 6h to fully dissolve it, centrifuge it at 10000r / min for 5min, and the supernatant obtained is the wool protein solution;

[0050] b. Add 6 g of lipoic acid powder to the wool protein solution obtained in step a, stir and react at 40° C. for 1 h to obtain a modified wool protein solution, then put it into a dialysis bag, and perform dialysis with deionized water as the dialysis fluid. Change the deionized water every 30 min, and continue dialysis for 4 h;

[0051] c. Add 0.2 g of Fe(NO3)3·9H2O to the modified wool protein solution after dialyzation in step b, stir at 40°C for 4 h, and freeze-dry the solution at -50°C for 12 h to obtain a protein gel;

[0052] d. The protein gel was calcined in a tubular furnace at 900° C. for 2 h. After calcination, it was acid-washed in a 0.3 mol / L HCl solution for 24 h, then washed with deionized water and dried to obtain a single-atom iron catalyst.

[0053] Example 4

[0054] An iron atom catalyst, the preparation operation of which is carried out according to the following steps:

[0055] a. Weigh 1g of wool and add it to 10mL of 120g / L tri(2-carboxyethyl)phosphine hydrochloride solution, treat it at 70℃ for 2h, add the treated wool fiber to 40mL of formic acid, stir it at 70℃ for 6h to fully dissolve it, centrifuge it at 10000r / min for 5min, and the supernatant obtained is the wool protein solution;

[0056] b. Add 3 g of lipoic acid powder to the wool protein solution obtained in step a, stir and react at 50° C. for 2 h to obtain a modified wool protein solution, then put it into a dialysis bag, and perform dialysis with deionized water as the dialysis fluid. Change the deionized water every 30 min, and continue dialysis for 4 h;

[0057] c. Add 0.15 g of FeCl3·6H2O to the modified wool protein solution after dialyzation in step b, stir at 40°C for 4 h, and freeze-dry the solution at -50°C for 15 h to obtain a protein gel;

[0058] d. Calcine the protein gel at 900° C. in a tube furnace for 3 h, then acid-wash it in a 0.3 mol / L HCl solution for 24 h, then wash it with deionized water and dry it to obtain a single-atom iron catalyst.

[0059] Example 5

[0060] An iron atom catalyst, the preparation operation of which is carried out according to the following steps:

[0061] a. Weigh 1g of wool and add it to 10mL of 120g / L tri(2-carboxyethyl)phosphine hydrochloride solution, treat it at 70℃ for 2h, add the treated wool fiber to 30mL of formic acid, stir it at 60℃ for 6h to fully dissolve it, centrifuge it at 10000r / min for 5min, and the supernatant obtained is the wool protein solution;

[0062] b. Add 0.5 g of lipoic acid powder to the wool protein solution obtained in step a, stir and react at 50° C. for 2 h to obtain a modified wool protein solution, then put it into a dialysis bag and perform dialysis with deionized water as the dialysis fluid. Change the deionized water every 30 min and continue for 4 h to complete the dialysis.

[0063] c. Add 0.15 g Fe(NO3)3·9H2O to the modified wool protein solution after dialyzation in step b, stir at 40°C for 4 h, and then freeze-dry the solution at -40°C for 12 h to obtain a protein gel.

[0064] d. Calcine the protein gel at 900°C in a tubular furnace for 2 h, then acid-wash it in a 0.3 mol / L HCl solution for 24 h, then wash it with deionized water and dry it to obtain a single atom catalyst.

[0065] The single-atom iron catalysts prepared in Examples 1 to 5 were used to perform an experiment on the degradation of p-chlorophenol by persulfate activation, and the performance of each catalyst was reflected by the experimental results.

[0066] Experiment: reaction temperature 25℃, catalyst addition amount 0.005g / L (in terms of Fe), initial p-chlorophenol mass concentration 20mg / L, peroxymonosulfate addition amount 0.2g / L, initial solution pH 6.8. Take 50mL p-chlorophenol solution in a beaker, add catalyst, stir for 30min to reach adsorption-desorption equilibrium, add peroxymonosulfate to start the reaction, and react for 60min; take samples at regular intervals, add 20μL sodium thiosulfate solution to terminate the reaction, filter with 0.22μm filter membrane and wait for testing, and the p-chlorophenol degradation effect is analyzed by gas chromatography.

[0067] The degradation effect of para-chlorophenol is characterized by "removal rate (R, %)", and the removal rate calculation formula is as follows:

[0068] R=((C0-C t ) / C0)×100%

[0069] Where: C0—initial substrate concentration, mg / L; Ct—substrate concentration at time t, mg / L.

[0070] The experimental results are shown in Table 1 below:

[0071] Table 1

[0072] catalyst Example 1 Example 2 Example 3 Example 4 Example 5 <![CDATA[Initial concentration C0 (mg / L)]]> 20.0 20.0 20.0 20.0 20.0 <![CDATA[Concentration C at time t (30 min) t (mg / L)]]> <0.1 0.4 0.5 0.6 1.6 Removal rate of parachlorophenol (%) >99 98 98 97 92 Reaction time (min) 30 30 30 30 30

[0073] Example 1 Catalytic results are as follows Figure 5 and 6As shown, the peak of p-chlorophenol was observed to be relatively high when the initial reaction solution was analyzed; after 30 minutes of reaction, the peak of p-chlorophenol basically disappeared, indicating that the catalyst had a high catalytic efficiency, the sulfate radicals obtained by activation had a high removal rate for p-chlorophenol, and the overall catalytic efficiency was high.

[0074] In addition, the catalyst of Example 1 was subjected to a cycle experiment, that is, after completing the activation persulfate degradation experiment for p-chlorophenol, the catalyst was recovered and activated at 300° C. for 1 h under a N2 atmosphere, and then used again to catalyze the persulfate activation degradation experiment for p-chlorophenol. The cycle experiment was repeated 5 times. The results are shown in Table 2 below.

[0075] Table 2

[0076]

[0077] It can be seen from the results in the above table that the wool protein-supported iron single-atom catalyst of the present invention has good stability when used sequentially.

[0078] Comparative Example 1

[0079] The single-atom iron catalyst of this comparative example did not use the modifier thioctic acid, but added the pore-forming agent ZnCl2, and was specifically prepared as follows.

[0080] Weigh 1g of wool and add it to 10mL of 120g / L tri(2-carboxyethyl)phosphine hydrochloride solution, treat it at 70℃ for 2h, add the treated wool fiber to 30mL of formic acid, stir it at 70℃ for 6h to fully dissolve, centrifuge it at 10000r / min for 5min, and the supernatant obtained is the wool protein solution, which is then placed in a dialysis bag and dialyzed with deionized water as the dialysis fluid. The deionized water is changed every 30min, and the dialysis is completed for 4h. Add 0.15gFe(NO3)3·9H2O and 13.6mg ZnCl2 to the dialyzed solution, where ZnCl2 is a pore-forming agent to increase the specific surface area of ​​the catalyst. After stirring at 40℃ for 4h, the solution is freeze-dried at -40℃ for 12h to obtain a protein gel. The protein gel was calcined at 900° C. in a tube furnace for 2 h, then acid-washed in a 0.3 mol / L HCl solution for 12 h, then washed with deionized water and dried to obtain a single-atom iron catalyst.

[0081] Comparative Example 2

[0082] The single-atom iron catalyst of this comparative example uses silk (silk fibroin) instead of wool (wool protein) as a carrier, does not use the modifier lipoic acid, and adds the pore-forming agent ZnCl2. The specific preparation is as follows.

[0083] Boil 1g of silk in 100mL of 0.2mol / L Na2CO3 aqueous solution for 3h to fully degummed the silk. Then add the degummed silk fibroin into 100ml of 9.3mol / L lithium bromide solution and stir at 65℃ for 2h. Finally, place the treated silk fibroin solution in a dialysis bag for 3 days. Add 0.15g Fe(NO3)3·9H2O and 13.6mg ZnCl2 to the dialyzed solution, where ZnCl2 is a pore-forming agent to increase the specific surface area of ​​the catalyst. After stirring at 40℃ for 4h, freeze-dry the solution at -40℃ for 12h to obtain a protein gel. Calcine the protein gel, place it in a tube furnace at 900℃ for 2h, then acid-wash it in 0.3mol / L HCl for 12h, then wash it with deionized water and dry it to obtain a single-atom iron catalyst.

[0084] Comparative Example 3

[0085] The catalyst of this comparative example is FeCl3·6H2O.

[0086] The catalysts of Comparative Examples 1 to 3 were respectively subjected to the persulfate activation and degradation of p-chlorophenol experiment. The persulfate activation and degradation of p-chlorophenol experiment was performed in the same manner as above. The experimental results are shown in Table 3 below:

[0087] Table 3

[0088] catalyst Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Initial concentration C0 (mg / L)]]> 20 20 20 <![CDATA[Concentration C at time t (30 min) t (mg / L)]]> 3.4 5.6 4.2 Removal rate of parachlorophenol (%) 83 72 79 Reaction time (min) 30 30 30

[0089] As shown in Table 3 above, the removal rate of para-chlorophenol by activated persulfate in the comparative example is low. After analysis, the catalytic efficiency of the catalyst in comparative example 1 is low because the modifier thioctic acid is not used. The specific surface area of ​​the catalyst is increased by the pore-forming agent zinc chloride, which reduces the coordination of sulfur and reduces the activity of Fe. At the same time, a porous structure such as Example 1 cannot be formed, resulting in a small specific surface area and insufficient contact with persulfate. The catalytic efficiency of the catalyst in comparative example 2 is low because the sulfur element in silk fibroin is less than wool protein, and N and S co-coordination cannot be formed. Its activity is lower than that in comparative example 1, reflecting the important role of sulfur coordination in improving catalytic activity. The trivalent iron ion of comparative example 3 is directly used for catalytic activation of persulfate, which is inefficient and cannot be recovered or recycled.

[0090] In summary, the wool protein carbon-supported single-atom iron catalyst modified with lipoic acid of the present invention utilizes nitrogen and sulfur in wool protein and sulfur-complexed iron ions in lipoic acid, and then prepares a carbon-supported single-atom iron structure anchored by sulfur and nitrogen through high-temperature calcination, so that the catalyst has the advantages of high activity, high stability, low cost and simple operation, and is applied to catalyze the activation and degradation of organic pollutants by persulfate, which can greatly improve the adsorption and catalytic efficiency.

Claims

1. A single-atom iron catalyst for degradation of organic pollutants by persulfate method, Features: The single-atom iron catalyst is a wool protein carbon-loaded asymmetric coordination single-atom iron catalyst, which is prepared by dissolving a wool protein solution through reduction pretreatment-formic acid method, modifying it with lipoic acid, then complexing it with iron ions, and finally freeze-drying, high-temperature calcining, and acid washing.

2. The single-atom iron catalyst for degrading organic pollutants by the persulfate method according to claim 1, Features: The wool protein solution is prepared by adding wool into a tri(2-carboxyethyl)phosphine hydrochloride solution, treating the wool at 70-90° C., and then adding the treated wool fibers into formic acid to fully dissolve the wool fibers.

3. The single-atom iron catalyst for degrading organic pollutants by the persulfate method according to claim 2, Features: The wool protein complexed iron ion modified with lipoic acid is prepared by adding lipoic acid powder to a wool protein solution, stirring the solution at 30-50°C, then dialyzing the solution, adding an iron precursor, and stirring the solution at 30-40°C.

4. The single-atom iron catalyst for degrading organic pollutants by persulfate method according to claim 3, Features: The amount of wool is 1-2 g, the concentration of tri(2-carboxyethyl)phosphine hydrochloride solution is 80-120 g / L, the amount is 10-50 mL, the amount of formic acid is 20-50 mL, the amount of lipoic acid is 0.5-10 g, and the amount of iron precursor is 0.1-0.2 g.

5. The single-atom iron catalyst for degrading organic pollutants by persulfate method according to claim 3, Features: The iron precursor is selected from at least one of ferric acetylacetonate, ferric chloride, ferrous chloride, ferrous nitrate, ferric sulfate and ferrous sulfate.

6. The single-atom iron catalyst for degrading organic pollutants by persulfate method according to claim 1, Features: The freeze drying temperature is -40 to -60°C; the high temperature calcination temperature is 700 to 1000°C; and the pickling uses HCl solution.

7. The preparation of the single-atom iron catalyst for degradation of organic pollutants by the persulfate method according to any one of claims 1 to 6, It is characterized in that The method comprises the following preparation steps: a. Add 1-2 g of wool to 10-50 mL of 80-120 g / L tris(2-carboxyethyl)phosphine hydrochloride solution, treat at 70-90° C. for 1-3 h to obtain wool fiber, add the wool fiber to 20-50 mL of formic acid, stir at 50-70° C. for 4-6 h to fully dissolve, centrifuge, and obtain the supernatant as the wool protein solution; b. Add 0.5-10 g of lipoic acid powder to the wool protein solution, stir and react at 30-50° C. for 1-3 h to obtain a modified wool protein solution, put it into a dialysis bag, and perform dialysis with deionized water; c. Add 0.1-0.2 g of iron precursor to the dialyzed modified wool protein solution, stir at 30-40° C. for 1-6 h, and freeze-dry the resulting solution at -40--60° C. for 12-48 h to obtain a protein gel; d. Calcine the protein gel at 700-1000° C. for 1-4 h, and then wash the calcined product with HCl solution, wash with water, and dry to obtain a single-atom iron catalyst.

8. The method for preparing the single-atom iron catalyst for degrading organic pollutants by the persulfate method according to claim 7, Features: In step a, the centrifugal speed is 10000 r / min and the time is 5 min; and / or; In step b, the dialysis treatment is performed by replacing deionized water every 30 to 40 minutes for 3 to 4 hours; and / or; In step d, the calcination temperature is 800-900° C. and the time is 1-3 hours; and / or; The calcined product is acid-washed in a 0.2-0.6 mol / L HCl solution for 12-24 h, then washed with deionized water and dried.

9. Use of the single-atom iron catalyst for degradation of organic pollutants by the persulfate method as claimed in any one of claims 1 to 6, Features: The single-atom iron catalyst is used as a catalyst for activating persulfate, and is used to replace the soluble iron salt catalyst used in the persulfate advanced oxidation process.

10. Use of the single-atom iron catalyst for degradation of organic pollutants by persulfate method according to claim 9, Features: Single-atom iron catalysts are suitable for acidic or alkaline reaction systems and can be recycled and repeatedly used in persulfate advanced oxidation processes.

Citation Information

Patent Citations

  • Collagen-based carbon material supported metal cobalt catalyst and preparation method and application thereof

    CN112169798A

  • Keratin regenerated material with sulfydryl / disulfide bond dynamic covalent cross-linking system and preparation method of keratin regenerated material

    CN116655939A

  • Use of heterocyclic disulfide compound as an agent for treating keratin fibers, such as hair, where the disulfide compound is associated with reducing agent

    FR2939671A1