Method for preparing porous carbon-loaded Ni-based catalyst from lignin residues and application of porous carbon-loaded Ni-based catalyst in hydrogenation of 5-hydroxymethylfurfural and furfural

By preparing porous carbon-supported nickel hydroxide-based catalysts from lignin residues during the comprehensive utilization of ligno fibers, the problems of harsh reaction conditions and polluted waste are solved, high-concentration hydrogenation reaction is achieved, and the utilization of biomass resources is improved. Efficiency and economic value are in line with the green and sustainable development goals.

CN118892834AActive Publication Date: 2024-11-05XIAMEN UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410937767.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

In the comprehensive utilization of wood fibers, there are problems of harsh reaction conditions and the production of large amounts of polluted waste. In the prior art, the reaction concentration of HMF and FF hydrogenation to prepare BHMF and FA is low, making it difficult to achieve the comprehensive utilization of biomass resources.

Method used

Porous carbon-supported nickel hydroxide-based catalysts are prepared by using lignin residues, nickel nitrate hexahydrate and sodium gluconate in hydrothermal method, and the temperature and hydrogen pressure conditions are optimized to prepare Ni/C catalysts with high specific surface area for high bottoms The selective hydrogenation reaction of 5-hydroxymethylfurfural and furfural is catalyzed at the substance concentration.

Benefits of technology

It has achieved high concentration hydrogenation reaction, reduced environmental pollution, improved the economic value of biomass, conformed to the development goals of green and sustainable chemistry, and has industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892834A_ABST
    Figure CN118892834A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a porous carbon loaded Ni-based catalyst from biomass lignin residues and the field of catalysis of 5-hydroxymethylfurfural and furfural, and discloses a method for preparing a porous carbon loaded Ni-based hydrogenation catalyst from lignin residues and application of the catalyst to selective hydrogenation of 5-hydroxymethylfurfural and furfural under high substrate concentration catalysis. A carbon material loaded nickel hydroxide-based catalyst precursor is prepared from lignin residues, nickel nitrate hexahydrate, sodium gluconate and water through a one-pot hydrothermal method, a Ni / C catalyst with a high specific surface area is obtained through high-temperature reduction, and the high-specific-surface-area Ni / C catalyst is obtained by optimizing the temperature, hydrogen pressure, reaction time and the like. The Ni / C catalyst can be used for catalyzing selective hydrogenation of 5-hydroxymethylfurfural and furfural under high substrate concentration. According to the preparation method of the catalyst, waste generated in the biomass conversion process is fully utilized, the problem of environmental pollution is solved, the overall economic value of biomass can be improved, comprehensive utilization of resources is achieved, and great industrial application value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomass resource utilization, and in particular to a method for preparing a porous carbon-supported Ni-based catalyst using lignin residue (solid residue from hydrolysis of corn cobs) and an application of the catalyst in catalyzing the hydrogenation of 5-hydroxymethylfurfural (HMF) and furfural (FF). Background Art

[0003] Lignocellulose has a complex and stable structure, containing multiple components such as lignin, cellulose, and hemicellulose [Mika LT, et al., Catalytic conversion of carbohydrates to initial platform chemicals: chemistry and sustainability [J]. Chemical reviews, 2018, 118 (2): 505-613.; Hou Qidong, et al., Biorefinery roadmap based on catalytic production and upgrading 5-hydroxymethylfurfural. Green Chemistry, 2021, 23 (1): 119-231.]. In the process of comprehensive utilization of lignocellulose, there are problems such as harsh reaction conditions (strong acid or strong alkali) and the generation of a large amount of polluted waste (waste liquid and solid residue). For example, after using corn cobs to hydrolyze to produce high-value-added chemicals, a large amount of lignin solid residue remains. How to maximize the pollution-free utilization of biomass resources, improve the overall economic value of biomass, and achieve comprehensive utilization of resources is an urgent problem to be solved.

[0004] Furan dimethanol (BHMF) and furfuryl alcohol (FA) can be produced by hydrogenating biomass platform molecules 5-hydroxymethylfurfural and furfural. They can be used as precursors for a variety of chemicals, such as polyesters, polyethers, fungicides, furan resins, etc. They can also be used as precursors for fuel additives (DMF, 2-MF), etc.

[0005] There are a large number of literatures and patents that have studied and reported on the hydrogenation of HMF and FF to prepare BHMF and FA (Maki-Arvela, et al., Catalytic hydrogenation / hydrogenolysis of 5-hydroxymethylfurfural to 2,5-dimethylfuran. Chemsuschem 2021, 14(1), 150-168.; Vikanova, K. et al., Advanced room-temperature synthesis of 2,5-bis(hydroxymethyl)furan—a monomer for biopolymers—from 5-hydroxymethylfurfural. ACS Sustainable Chemistry&Engineering2021,9(3),1161-1171.Wang,Q.;Santos,S.;Urbina-Blanco,CA;Zhou,W.;Yang,Y.;Mar inova,M.;Heyte,S.;Joelle,T.-R.;Ersen,O.;Baaziz,W.;Safonova,OV;Saeys,M.;Ordomsky,VV,Ru(III)single site solid micellar catalyst for selective aqueous phasehydrogenation of carbonyl groups in biomass-derived compounds.AppliedCatalysis B:Environmental 2022,300,120730. Method for producing BHMF, BHMTHF, HDO and HTO from HMF: CN107001197B; Method for hydrogenating furfural to furfuryl alcohol: CN115974820B), but the problem of low reaction concentration is common. Therefore, using biomass reaction solid residue as a raw material for preparing catalyst for high-concentration hydrogenation of HMF and FF to prepare BHMF and FA can realize the comprehensive utilization of biomass resources, which is of great significance to green and sustainable development. Summary of the invention

[0006] To solve the problems existing in the above-mentioned prior art, the present invention provides a method for preparing a porous carbon-supported Ni-based hydrogenation catalyst from lignin residue and an application of catalyzing the selective hydrogenation of 5-hydroxymethylfurfural and furfural at a high substrate concentration. A carbon material-supported nickel hydroxide-based catalyst precursor is prepared by a one-pot hydrothermal method using lignin residue (solid residue from hydrolysis of corn cobs), nickel nitrate hexahydrate, sodium gluconate and water, and a high-specific surface area Ni / C catalyst is obtained by high-temperature reduction. By optimizing temperature, hydrogen pressure, reaction time, etc., the Ni / C catalyst can be used to catalyze the selective hydrogenation of 5-hydroxymethylfurfural and furfural at a high substrate concentration. The catalyst preparation method in the present invention makes full use of the waste generated in the biomass conversion process, not only reduces environmental pollution problems, but also improves the overall economic value of biomass, realizes the comprehensive utilization of resources, meets the development goals of green sustainable chemistry, and has great industrial application value.

[0007] In order to achieve the above object, the present invention provides a carbon-supported nickel-based catalyst prepared by the following method:

[0008] (1) Weigh a certain amount of lignin residue, nickel nitrate hexahydrate, and sodium gluconate in deionized water, then transfer them into a sealed high-pressure reactor, heat them to 160-200°C under magnetic stirring, and keep them for 15-30 hours. After cooling to room temperature, filter under reduced pressure, wash the filter cake, and dry it at 60-100°C in vacuum to obtain a solid named Ni(OH) 2 / C. The addition ratio of the lignin residue, nickel nitrate hexahydrate, sodium gluconate and deionized water is (4-10) g: (3-8) g: (4-10) g (120-300) mL.

[0009] (2) The catalyst precursor (Ni(OH) 2 / C), and then subjected to programmed temperature reduction in a hydrogen atmosphere to obtain a porous carbon-supported nickel-based catalyst (Ni / CT, where T represents the reduction temperature, such as 350, 400, 500, or 600°C).

[0010] The invention is characterized in that the addition ratio of the lignin residue, nickel nitrate hexahydrate, sodium gluconate and deionized water is (6-8) g: (4-6) g: (5-8) g (150-250) mL.

[0011] Furthermore, the heating temperature in step (1) is 180° C. and maintained for 24 hours.

[0012] Furthermore, the retention time in step (1) is 24 hours.

[0013] Furthermore, the reduction process in step (2) is: heating to 350-600°C at 5°C / min in a tubular furnace with hydrogen, keeping the temperature for 2-4h, and then naturally cooling to room temperature.

[0014] Preferably, the temperature is raised to 500° C. at 5° C. / min in a tubular furnace filled with hydrogen, kept at that temperature for 2 h, and then naturally cooled to room temperature.

[0015] The present invention also provides an application of the porous carbon-supported nickel-based (Ni / CT) catalyst in the hydrogenation of 5-hydroxyfurfural and furfural to prepare furan dimethanol and furfuryl alcohol.

[0016] It is characterized by comprising the following steps:

[0017] Add catalyst (Ni / CT) (0.02-0.2) g and 3 ml of 5-hydroxymethylfurfural aqueous solution (4-20 wt / %) into a high-pressure reactor, seal the reactor, fill it with 10 bar-40 bar of hydrogen, and react for 1-5 hours at 30-100° C. with magnetic stirring at 300-800 rpm to obtain furandimethanol.

[0018] Add catalyst (Ni / CT) (0.02-0.2) g and 3 ml of furfural aqueous solution (20 wt / %) into a high-pressure reactor, seal the reactor, fill it with 10 bar-20 bar of hydrogen, and react for 1-5 hours at 30-100° C. with magnetic stirring at 300-800 rpm to obtain furfural alcohol and tetrahydrofurfuryl alcohol.

[0019] Compared with the prior art, the present invention has the following advantages and effects: the present invention comprehensively utilizes biomass reaction residues as carriers to prepare highly dispersed small-particle nickel-based catalysts, and prepares high specific surface area Ni / C catalysts by high-temperature calcination reduction. Not only can the problem of solid residues generated during biomass conversion be reduced, but also the comprehensive utilization of biomass resources can be achieved, and the overall economic value of biomass can be improved. The present invention uses the above-prepared catalyst for high-concentration selective hydrogenation of 5-hydroxymethylfurfur and furfural. In addition, the catalyst preparation process of the present invention is simple, low-cost, and conducive to large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The X-ray diffraction patterns (XRD patterns) of the lignin solid residue and the prepared catalyst precursor in Example 1 are shown in FIG.

[0021] Figure 2 This is the X-ray diffraction pattern (XRD pattern) of the carbon-supported nickel-based catalyst (Ni / CT, T represents the reduction temperature: 350, 400, 500, 600) prepared in Example 1.

[0022] Figure 3 The carbon-supported nickel-based catalyst (Ni / CT, T represents the reduction temperature: 350, 400, 500, 600) prepared in Example 1 is N 2 Adsorption-desorption curves.

[0023] Figure 4 This is a scanning electron microscope image (SEM) of the carbon-supported nickel-based catalyst (Ni / C-500) prepared in Example 1.

[0024] Figure 5 This is the Ni2p spectrum of the carbon-supported nickel-based catalyst (Ni / C-500) prepared in Example 1. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and the accompanying drawings of the specification, but the following embodiments are not intended to limit the scope of protection claimed in the present invention.

[0026] Unless otherwise specified, the reagents and instruments used in the following examples are commercially available products. Specific implementation examples are as follows:

[0027] Example 1: A porous carbon-supported nickel-based catalyst (Ni / CT) was prepared by the following method:

[0028] Weigh 7g of lignin residue, 5.8g of nickel nitrate hexahydrate, and 6g of sodium gluconate in 200ml of deionized water, then transfer them into a sealed autoclave, heat to 180°C under magnetic stirring, and keep for 24h. After cooling to room temperature, filter under reduced pressure, wash the filter cake, and dry it at 70°C in vacuum to obtain a solid named Ni(OH) 2 / C. Then Ni(OH) 2 / C, in a hydrogen atmosphere, the temperature was raised to 500°C at 5°C / min, kept for 2 h, and naturally cooled to room temperature to obtain Ni / C-500 catalyst. According to the same method, the calcination temperature was changed to obtain a series of Ni / CT catalysts (T represents the reduction temperature: 350, 400, 500, 600).

[0029] The biomass solid reaction residue used in Example 1 and the prepared catalyst precursor (Ni(OH) 2 / C) for X-ray diffraction (XRD) analysis, such as Figure 1 As shown, the biomass solid residue contains a certain amount of silica impurities. After high-temperature loading, new diffraction peaks are generated, indicating that Ni-related substances are successfully loaded onto the carrier.

[0030] Figure 2 This is the X-ray diffraction pattern (XRD pattern) of the Ni / CT series catalyst prepared in Example 1. When the catalyst is calcined and reduced at 350°C, there is no obvious nickel-related diffraction peak in the diffraction pattern of the Ni / C-350 catalyst. As the calcination temperature increases, the Ni species is reduced to Ni 0, 2θ=44.4°, 51.7°, 75.9° correspond to Ni 0 (111), (200) and (220) crystal planes (PFD:04-002-77521). As the calcination temperature increases, the crystallinity of Ni increases. 2 Adsorption-desorption curve ( Figure 3 ) Analysis shows that the specific surface area of ​​Ni / C-500 is 320m 2 / g. SEM shows that the surface of Ni / C-500 catalyst is rough and contains a lot of wrinkles, which may be one of the reasons why Ni / C-500 has a large specific surface area, increasing the contact probability between the substrate and the active center, which may be the reason why Ni / C-500 catalyst has high activity ( Figure 4 ).

[0031] Figure 5 This is the Ni2p diagram of the X-ray photoelectron spectroscopy (XPS) of Ni / C-500 prepared in Example 1. At 500°C, the Ni in the catalyst was almost completely reduced to Ni 0 , which is consistent with the XRD data.

[0032] Embodiment 2-4

[0033] A series of Ni-based catalysts (Ni / CT, T represents the reduction temperature: 350, 400, 500, 600° C.) prepared in Example 1 were used for selective hydrogenation of HMF to prepare BHMF, the steps being:

[0034] Ni / CT catalyst (0.04 g) and 3 mL of 5-hydroxymethylfurfural aqueous solution (4 wt%) were added to a high pressure reactor, the air in the reactor was replaced with hydrogen, and the reaction was heated to 50° C. at a stirring speed of 500 rpm for 1 h, cooled to room temperature, and the reaction solution was detected by liquid chromatography (Agilent-1260 Infinity II). Examples 2-5 show that the catalyst calcination temperature is closely related to the selectivity of BHMF, and the catalyst calcined at 500° C. has the best BHMF selectivity (91%).

[0035] Table 1

[0036]

[0037] Embodiment 6-9

[0038] The catalyst Ni / C-500 in Example 4 was used as the catalyst for subsequent research. The reaction temperature has a significant effect on the conversion rate of HMF and the selectivity of BHMF. As the temperature increases, the conversion rate of HMF increases, and the selectivity of BHMF increases first and then decreases, which is related to the excessive hydrogenation of BHMF at high temperature. 50°C is the optimal temperature for preparing BHMF, and 50°C is used to further optimize the hydrogen pressure and reaction time.

[0039] Table 2

[0040]

[0041] Examples 10-13

[0042] The selective hydrogenation of HMF is a three-phase reaction of gas, solid and liquid. The greater the hydrogen pressure, the more hydrogen dissolved in the solution. Experimental data show that hydrogen pressure has a significant effect on BHMF. The higher the hydrogen pressure, the more BHMF over-hydrogenation products and the lower the selectivity of BHMF. At 2MPa, the selectivity of BHMF is 91%.

[0043] Table 3

[0044]

[0045] Examples 14-18

[0046] The effect of reaction time on the selective hydrogenation of HMF to prepare BHMF was further studied. As shown in Examples 14-18, with the increase of reaction time, the conversion rate of HMF gradually increased. When the reaction time was 5 min, the conversion rate of HMF was 15%. As the reaction time was extended to 60 min, HMF was basically completely converted, and the BHMF selectivity was 91%.

[0047] Table 4

[0048]

[0049] Embodiment 19

[0050] Ni / C-500 catalyst (0.095 g) and 3 mL of 5-hydroxymethylfurfural aqueous solution (10 wt%) were added to a high pressure reactor. After the reactor was sealed, the air in the reactor was replaced with hydrogen for 5-6 times, and 2 MPa of hydrogen was filled in. The reaction was stirred at 500 rpm and reacted at 50° C. for 2 h. The reaction solution was cooled to room temperature and detected by liquid chromatography (Agilent-1260 Infinity II). The calculated HMF conversion rate was 69%, and the BHMF selectivity was 84%.

[0051] Embodiment 20

[0052] Ni / C-500 catalyst (0.19 g) and 3 mL of 5-hydroxymethylfurfural aqueous solution (20 wt%) were added to a high pressure reactor. After the reactor was sealed, the air in the reactor was replaced with hydrogen for 5-6 times, and 2 MPa of hydrogen was filled in. The reaction was carried out at 50° C. for 4 h under stirring at 500 rpm, and the reaction was cooled to room temperature. The solution after the reaction was detected by liquid chromatography (Agilent-1260 Infinity II). The calculated HMF conversion rate was >99%, and the BHMF selectivity was 90%.

[0053] Embodiment 21

[0054] Ni / C-500 catalyst (0.25 g) and 3 mL of furfural aqueous solution (20 wt%) were added to a high pressure reactor. After the reactor was sealed, the air in the reactor was replaced with hydrogen for 5-6 times, and 2 MPa of hydrogen was filled in. The reactor was stirred at 500 rpm and reacted at 50°C for 2 h. The reaction solution was cooled to room temperature and detected by liquid chromatography (Agilent-1260 Infinity II). The furfural conversion rate was calculated to be >97%, the selectivity of furfuryl alcohol was 67%, and the selectivity of tetrahydrofurfural was 13%.

[0055] Embodiment 22

[0056] Ni / C-500 catalyst (0.25 g) and 3 mL of furfural aqueous solution (20 wt%) were added to a high pressure reactor. After the reactor was sealed, the air in the reactor was replaced with hydrogen for 5-6 times, and 2 MPa of hydrogen was filled in. The reactor was stirred at 500 rpm and reacted at 50°C for 4 hours. The reaction solution was cooled to room temperature and detected by liquid chromatography (Agilent-1260 Infinity II). The furfural conversion rate was calculated to be >99%, the selectivity of furfuryl alcohol was 47%, and the selectivity of tetrahydrofurfural was 37%.

[0057] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A porous carbon-supported Ni-based catalyst prepared from lignin residue is prepared by the following method: (1) Weighing lignin residue (e.g., solid residue from hydrolysis of corn cobs), nickel nitrate hexahydrate, and sodium gluconate in deionized water, then transferring the mixture into a sealed autoclave, heating the mixture to 160-200° C. under magnetic stirring, and retaining the mixture for 15-30 hours; cooling the mixture to room temperature, filtering the mixture under reduced pressure, washing the filter cake, and drying the mixture under vacuum at 60-100° C. to obtain a solid catalyst precursor Ni(OH)2 / C; The addition ratio of lignin residue, nickel nitrate hexahydrate, sodium gluconate and deionized water is (4-10 g:(3-8) g:(4-10) g (120-300) mL; (2) reducing the catalyst precursor Ni(OH)2 / C obtained in step (1) by programmed temperature reduction in a hydrogen atmosphere to obtain a porous carbon-supported nickel-based catalyst Ni / CT; in, T represents the reduction temperature, for example 350-600°C, specifically 350, 400, 500, 600°C.

2. The catalyst according to claim 1, characterized in that: The addition ratio of the lignin residue, nickel nitrate hexahydrate, sodium gluconate and deionized water is (6-7) g: (4-6) g: (5-8) g (150-250) mL.

3. The catalyst according to claim 1, characterized in that: In step (1), the heating temperature is 180° C. and maintained for 24 hours.

4. The catalyst according to claim 1 or 2, characterized in that: The reduction process in step (2) is as follows: heating to 350-600° C. at 5° C. / min in a tubular furnace filled with hydrogen, and keeping the temperature for 2 h to obtain a porous carbon-supported nickel-based catalyst Ni / CT.

5. Use of the porous carbon-supported nickel-based catalyst according to any one of claims 1 to 4 in the hydrogenation of 5-hydroxyfurfural and the catalytic preparation of furandimethanol and furfural from furfural.

6. A method for preparing furandimethanol by hydrogenating 5-hydroxyfurfural, characterized in that: The steps include: Add catalyst Ni / CT and 5-hydroxymethylfurfural aqueous solution into a high-pressure resistant reactor, seal the reactor, fill it with 10 bar-40 bar hydrogen, and react for 1-5 hours at 30-100° C. with magnetic stirring at 300-800 rpm to obtain furandimethanol.

7. The method according to claim 6, characterized in that Add 0.02-0.2g of Ni / CT catalyst and 3ml of 4-20wt / % 5-hydroxymethylfurfural aqueous solution into a high-pressure reactor, seal the reactor, fill it with 10bar-40bar hydrogen, and react for 1-5h at 30-100°C with magnetic stirring at 300-800rpm to obtain furandimethanol.

8. A method for preparing furfuryl alcohol from furfural, characterized in that: The method comprises the following steps: adding a catalyst Ni / CT and a furfural aqueous solution into a high-pressure resistant reactor, sealing the reactor and filling it with 10 bar to 20 bar of hydrogen, and reacting for 1 to 5 hours at 30 to 100° C. under magnetic stirring at 300 to 800 rpm to obtain furfural alcohol.

9. The method according to claim 8, characterized in that Add 0.02-0.2 g of Ni / C-T catalyst and 3 ml of 20 wt / % furfural aqueous solution into a high-pressure reactor, seal the reactor, fill it with 10 bar-20 bar of hydrogen, and react for 1-5 hours at 30-100° C. with magnetic stirring at 300-800 rpm to obtain furfuryl alcohol.

Citation Information

Patent Citations

  • Methods for producing BHMF, BHMTHF, HDO and HTO from HMF

    CN107001197B

  • A method for preparing furfuryl alcohol by hydrogenating furfural

    CN115974820B

  • Biomass-based carbon material supported nano-nickel catalyst, preparation method and application thereof

    CN112844476A

  • Bio-based carbon supported catalyst and preparation method thereof

    CN114618468A

  • Synthesis of nano crystalline niobia / carbon composites with improved hydrothermal stability