A NiO@CuO / ZnO composite catalytic material and its preparation method and application
The activation of bisulfate by NiO@CuO/ZnO composite catalytic material solves the problem of poor removal of ciprofloxacin in traditional water treatment methods, and achieves efficient degradation and low-cost ciprofloxacin pollutant treatment. It is suitable for Wide range of water treatment applications.
Patent Information
- Application Number
- CN202411404207.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-10
AI Technical Summary
Traditional water treatment methods are not effective in removing drug contaminants such as ciprofloxacin, and a single transition metal oxide catalyst has problems with low catalytic efficiency and large metal ion dissolution.
The NiO@CuO/ZnO composite catalytic material was used to prepare the material by hydrothermal method, and it was used to activate the bisulfate to generate active radicals, thereby improving the degradation efficiency of ciprofloxacin.
It significantly improves the degradation efficiency of ciprofloxacin, and the degradation effect is effective within the pH range of 3 to 11, and the material is stable and repeatable, and the cost is low, which reduces secondary pollution.
Smart Images

Figure CN118892837B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and in particular relates to a NiO@CuO / ZnO composite catalytic material and a preparation method and application thereof. Background Art
[0002] Ciprofloxacin (CIP) is a fluoroquinolone antibiotic commonly used to treat bacterial infections in humans and livestock. Due to its widespread use by consumers and the fact that most CIP enters the environment through metabolism, CIP is frequently detected in a variety of water bodies, causing serious harm to the ecosystem. Studies have shown that traditional water treatment methods are ineffective in removing pharmaceutical contaminants. Therefore, it is particularly important to develop a new and efficient method for deep treatment of CIP in water.
[0003] Advanced Oxidation Process (AOP S ) based on the activation of persulfate (PMS) to generate sulfate radicals (SO 4 • - ) is a new technology for removing organic pollutants. Due to its asymmetric shape and other characteristics, PMS is believed to be easier to activate and better degrade difficult-to-degrade organic molecules. Among the many PMS activation methods, transition metal oxides can activate PMS at room temperature and have a good degradation effect on organic pollutants in water, while single transition metal materials often have problems with low catalytic efficiency or large leaching. In order to improve its catalytic degradation efficiency, a variety of composite catalyst materials have shown catalytic degradation performance and stability that are superior to single transition metal oxide catalysts. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a NiO@CuO / ZnO composite catalytic material.
[0005] Another object of the present invention is to provide a method for preparing the above-mentioned NiO@CuO / ZnO composite catalytic material.
[0006] Another object of the present invention is to provide an application of the above-mentioned NiO@CuO / ZnO composite catalytic material.
[0007] The present invention is achieved by providing a method for preparing a NiO@CuO / ZnO composite catalytic material, the method comprising the following steps:
[0008] (1) Put Ni (NO 3 ) 2 •6H 2 O, Cu (NO 3 ) 2 •3H 2O is dissolved in a mixed solution of deionized water and ethylene glycol to obtain solution A; thiourea is dissolved in a mixed solution of deionized water and ethylene glycol to obtain solution B; Zn(AC) 2 Dissolve in deionized water, then add thiourea to obtain solution C;
[0009] (2) Add solution B dropwise into solution A, stir vigorously, transfer into a high-pressure reactor, and perform a hydrothermal reaction at 160-200°C for 20-28 h. After the reaction is completed, centrifuge the reaction product to separate the hydrothermal product, wash and dry the hydrothermal product in sequence to obtain a precursor; ultrasonically mix the precursor with deionized water to obtain a precursor solution;
[0010] (3) adding solution C to the precursor solution and conducting a hydrothermal reaction at 120-160° C. for 6-10 h. After the reaction is completed, centrifuging the reaction product to obtain the hydrothermal product, and then drying, grinding, and calcining the hydrothermal product in sequence to obtain a NiO@CuO / ZnO composite catalytic material.
[0011] Preferably, in step (1), in the solution A, Ni(NO 3 ) 2 •6H 2 O, Cu (NO 3 ) 2 •3H 2 The molar volume ratio of O, deionized water, and ethylene glycol is 2~4 mmol:2~4 mmol:25 mL:25 mL;
[0012] In the solution B, the molar volume ratio of thiourea, deionized water, and ethylene glycol is 24 mmol:10 mL:10 mL;
[0013] In the solution C, the Zn(AC) 2 , deionized water, and thiourea have a molar volume ratio of 2 mmol:25 mL:2mmol.
[0014] Preferably, in step (2), the Ni(NO 3 ) 2 •6H 2 The molar ratio of O to thiourea in solution B is 2~4mmol:24mmol.
[0015] Preferably, in step (3), the precursor, Zn(AC) in solution C 2 The mass molar ratio is 0.1 g~0.3g:2 mmol.
[0016] Preferably, the Zn(AC) 2 、Cu(NO 3 ) 2•3H 2 The molar mass ratio of O and precursor is 2 mmol:3 mmol:0.2 g.
[0017] Preferably, in step (3), the calcination conditions are as follows: calcination temperature 600-1000°C, heating rate 5°C / min, and calcination time 1-3 h.
[0018] The invention further discloses a NiO@CuO / ZnO composite catalytic material prepared by the method.
[0019] The invention further discloses the application of the NiO@CuO / ZnO composite catalytic material in activating hydrogen persulfate to treat wastewater.
[0020] Preferably, the pollutants in the wastewater are antibiotic pollutants.
[0021] Preferably, the pH value of the wastewater is 3-11.
[0022] The present invention overcomes the shortcomings of the prior art and provides a NiO@CuO / ZnO composite catalytic material and its preparation method and application. The present invention is to compound the oxides of Cu, Ni and Zn transition metals. Among these transition metal oxides, NiO is a p-type semiconductor with low price, low toxicity and high content. CuO has various valence states (Cu 0 , Cu + and Cu 2+ ), with high catalytic efficiency in a wide pH range. The combination of CuO and NiO has a significant performance in activating PMS, showing excellent CIP degradation efficiency. ZnO is an n-type semiconductor with good electron transfer ability. The synergistic effect of Cu, Ni, and Zn promotes the transfer of electrons and better activates PMS to effectively degrade antibiotics.
[0023] Compared with the shortcomings and deficiencies of the prior art, the present invention has the following beneficial effects:
[0024] (1) The NiO@CuO / ZnO composite catalytic material of the present invention can activate hydrogen persulfate. The various material components in the NiO@CuO / ZnO composite catalytic material, such as NiO@CuO and ZnO, act together with PMS, and utilize the activation effect of NiO@CuO / ZnO on PMS to promote the generation of active free radicals and improve the degradation efficiency of antibiotic pollutants in water. In addition, the amount of metal ions dissolved in NiO@CuO / ZnO is small, which reduces secondary pollution, has good stability and repeatability, is low in cost, is easy to operate, and has a wide range of promotion and application prospects.
[0025] (2) The NiO@CuO / ZnO composite catalytic material of the present invention has a good removal effect on antibiotics in wastewater, is clean and pollution-free, and the NiO@CuO / ZnO composite catalytic material can degrade antibiotic wastewater with a wide pH value range, and the pH value range of the antibiotic wastewater can reach 3~11. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The XRD diffraction comparison patterns of the NiO@CuO / ZnO composite catalytic material of Example 1 of the present invention, the NiO@CuO of Comparative Example 2, and CuO;
[0027] Figure 2 This is a comparison chart of the degradation efficiency of ciprofloxacin (CIP) by different catalytic materials provided in Example 1 of the present invention and Comparative Examples 1 to 3;
[0028] Figure 3 This is the degradation diagram of ciprofloxacin (CIP) by NiO@CuO / ZnO composite catalytic material at different molar ratios of CuO and NiO;
[0029] Figure 4 It is the degradation diagram of ciprofloxacin (CIP) when each composite catalytic material is used as catalyst when NiO:CuO is 3:3 and ZnO mass ratio is different;
[0030] Figure 5 : is a graph showing the degradation of ciprofloxacin (CIP) by the NiO@CuO / ZnO composite catalytic material of Example 1 of the present invention at different dosages and different dosages of hydrogen persulfate; wherein, Figure 5 (a) is the degradation efficiency diagram of ciprofloxacin (CIP) at different dosages of NiO@CuO / ZnO composite catalytic materials. Figure 5 (b) is the degradation efficiency diagram of ciprofloxacin (CIP) at different dosages of PMS;
[0031] Figure 6 is a graph showing the degradation of ciprofloxacin (CIP) by the NiO@CuO / ZnO composite catalytic material provided in Example 1 of the present invention under the influence of different anions and humic acid; wherein, Figure 6 (a)~(d) are NO 3 - , Cl - , HCO 3 - and the degradation diagram of the effect of humic acid (HA) on ciprofloxacin (CIP);
[0032] Figure 7 This is a graph showing the degradation of ciprofloxacin (CIP) by the NiO@CuO / ZnO composite catalytic material provided in Example 1 of the present invention at different pH values. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0034] Example 1
[0035] (1) 3 mmol of Ni(NO 3 ) 2 •6H 2 O and 3 mmol Cu(NO 3 ) 2 •3H 2 O was dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A;
[0036] Dissolve 24 mmol of thiourea in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B;
[0037] Take 2 mmol of Zn(AC) 2 Place in a 100 mL beaker and add 25 mL of deionized water. Stir magnetically for 20-30 min. 2 When it is completely dissolved, add 2 mmol of thiourea to form solution C;
[0038] (2) Stir solution A and solution B on a magnetic stirrer for 20 min respectively, add solution B drop by drop into solution A, stir vigorously for 20 min, and then transfer to a high-pressure reactor for hydrothermal reaction. The hydrothermal time is 24 h and the temperature is 180°C. After the reaction is completed, the reaction product is cooled and centrifuged at high speed to obtain the hydrothermal product. The hydrothermal product is washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a drying oven for drying to obtain a precursor. Take 0.2 g of the precursor and put it into a 100 mL beaker and add 50 mL of deionized water. Perform ultrasonic treatment for 40 min to obtain a precursor solution.
[0039] (3) Pour solution C into the ultrasonic precursor material, stir magnetically for 20 min, transfer into a 100 mL stainless steel hydrothermal reactor with a polytetrafluoroethylene liner, and perform hydrothermal reaction at 140 °C for 8 h. After the reaction, cool the reaction product and centrifuge it at high speed to obtain the hydrothermal product. Wash the hydrothermal product with deionized water for 3 times and with anhydrous ethanol for 2 times, and finally dry it at 60 °C to obtain the composite material.
[0040] 0.2 g of the composite material was weighed and ground thoroughly, then placed in a porcelain boat, heated to 800 °C in a tube furnace at 5 °C / min, kept warm for 2 h, and naturally cooled to obtain a NiO@CuO / ZnO composite catalytic material with a molar ratio of NiO to CuO of 3:3, recorded as NiO@CuO (3:3)-0.2 g / ZnO.
[0041] Example 2
[0042] The preparation method is basically the same as that in Example 1, except that: Ni(NO 3 ) 2 •6H 2 O is 2 mmol, Cu(NO 3 ) 2 •3H 2 O is 4 mmol, and the molar ratio of NiO and CuO in the obtained material is 2:4, which is recorded as NiO@CuO (2:4)-0.2 g / ZnO.
[0043] Example 3
[0044] The preparation method is basically the same as that in Example 1, except that: Ni(NO 3 )2•6H 2 O is 4 mmol, Cu(NO 3 ) 2 •3H 2 O is 2 mmol, and the molar ratio of NiO and CuO in the obtained material is 4:2, which is recorded as NiO@CuO (4:2)-0.2 g / ZnO.
[0045] Example 4
[0046] The preparation method is basically the same as that in Example 1, except that the amount of the precursor used is 0.1 g, and a NiO@CuO / ZnO composite catalytic material with a molar ratio of NiO to CuO of 3:3 is obtained, which is recorded as NiO@CuO (3:3)-0.1 g / ZnO.
[0047] Example 5
[0048] The preparation method is basically the same as that in Example 1, except that the amount of the precursor used is 0.25 g, and a NiO@CuO / ZnO composite catalytic material with a molar ratio of NiO to CuO of 3:3 is obtained, which is recorded as NiO@CuO (3:3)-0.25 g / ZnO.
[0049] Example 6
[0050] The preparation method is basically the same as that in Example 1, except that the amount of the precursor used is 0.3 g, and a NiO@CuO / ZnO composite catalytic material with a molar ratio of NiO to CuO of 3:3 is obtained, which is recorded as NiO@CuO (3:3)-0.3 g / ZnO.
[0051] Example 7
[0052] (1) 2 mmol of Ni(NO 3 ) 2 •6H 2 O and 4 mmol Cu(NO 3 ) 2 •3H 2 O was dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A;
[0053] Dissolve 24 mmol of thiourea in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B;
[0054] Take 2 mmol of Zn(AC) 2 Place in a 100 mL beaker and add 25 mL of deionized water. Stir magnetically for 20-30 min. 2 When it is completely dissolved, add 2 mmol of thiourea to form solution C;
[0055] (2) Stir solution A and solution B on a magnetic stirrer for 20 min respectively, add solution B drop by drop into solution A, stir vigorously for 30 min, and then transfer to a high-pressure reactor for hydrothermal reaction. The hydrothermal time is 20 h and the temperature is 160 °C. After the reaction is completed, the reaction product is cooled and centrifuged at high speed to obtain the hydrothermal product. The hydrothermal product is washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a drying oven for drying to obtain a precursor; take 0.2 g of the precursor and put it into a 100 mL beaker and add 50 mL of deionized water. Perform ultrasonic treatment for 40 min to obtain a precursor solution;
[0056] (3) Pour solution C into the ultrasonic precursor material, stir magnetically for 30 min, transfer into a 100 mL stainless steel hydrothermal reactor with a polytetrafluoroethylene liner, and perform hydrothermal reaction at 120 °C for 6 h. After the reaction, cool the reaction product and centrifuge it at high speed to obtain the hydrothermal product. Wash the hydrothermal product with deionized water for 3 times and with anhydrous ethanol for 2 times, and finally dry it at 60 °C to obtain the composite material.
[0057] 0.2 g of the composite material was weighed and ground thoroughly, then placed in a porcelain boat, heated to 600 °C at 5 °C / min in a tube furnace, kept warm for 1 h, and cooled naturally to obtain a NiO@CuO / ZnO composite catalytic material.
[0058] Example 8
[0059] (1) 4 mmol of Ni(NO 3 ) 2 •6H 2 O and 2 mmol Cu(NO 3 ) 2 •3H 2 O was dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A;
[0060] Dissolve 24 mmol of thiourea in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B;
[0061] Take 2 mmol of Zn(AC) 2 Place in a 100 mL beaker and add 25 mL of deionized water. Stir magnetically for 20-30 min. 2 When it is completely dissolved, add 2 mmol of thiourea to form solution C;
[0062] (2) Stir solution A and solution B on a magnetic stirrer for 20 min respectively, add solution B drop by drop into solution A, stir vigorously for 30 min, and then transfer to a high-pressure reactor for hydrothermal reaction. The hydrothermal time is 28 h and the temperature is 200 °C. After the reaction is completed, the reaction product is cooled and centrifuged at high speed to obtain the hydrothermal product. The hydrothermal product is washed with deionized water and anhydrous ethanol for 3 times each, and then placed in a drying oven for drying to obtain a precursor. Take 0.2 g of the precursor and put it into a 100 mL beaker and add 50 mL of deionized water. Perform ultrasonic treatment for 40 min to obtain a precursor solution.
[0063] (3) Pour solution C into the ultrasonic precursor material, stir magnetically for 10 min, transfer into a 100 mL stainless steel hydrothermal reactor with a polytetrafluoroethylene liner, and perform hydrothermal reaction at 160 °C for 10 h. After the reaction, cool the reaction product and centrifuge it at high speed to obtain the hydrothermal product. Wash the hydrothermal product with deionized water 3 times and with anhydrous ethanol 2 times, and finally dry it at 60 °C to obtain the composite material.
[0064] 0.2 g of the composite material was weighed and ground thoroughly, then placed in a porcelain boat, heated to 800 °C at 5 °C / min in a tube furnace, kept warm for 2 h, and cooled naturally to obtain a NiO@CuO / ZnO composite catalytic material.
[0065] Comparative Example 1
[0066] (1) 6 mmol of Ni(NO 3 ) 2•6H 2 O was dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A;
[0067] Dissolve 24 mmol of thiourea in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B;
[0068] (2) Solution A and solution B were stirred on a magnetic stirrer for 20 min respectively, and solution B was dripped dropwise into solution A. After vigorous stirring for 20 min, the mixture was transferred into a high-pressure reactor for hydrothermal reaction at a temperature of 180 °C and a time of 24 h. After the reaction, a precursor was obtained.
[0069] (3) The obtained precursor was washed with deionized water and anhydrous ethanol three times each, and then placed in a drying oven for drying. The dried precursor was calcined in a tube furnace by increasing the temperature to 800 °C at 5 °C / min for 2 h to obtain NiO material.
[0070] Comparative Example 2
[0071] (1) 3 mmol of Ni(NO 3 ) 2 •6H 2 O and 3 mmol Cu(NO 3 ) 2 •3H 2 O was dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A;
[0072] Dissolve 24 mmol of thiourea in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B;
[0073] (2) Solution A and solution B were stirred on a magnetic stirrer for 20 min respectively, and solution B was dripped dropwise into solution A. After vigorous stirring for 20 min, the mixture was transferred into a high-pressure reactor for hydrothermal reaction at a temperature of 180 °C and a time of 24 h. After the reaction, a precursor was obtained.
[0074] (3) The obtained precursor was washed with deionized water and anhydrous ethanol three times each, and then placed in a drying oven for drying. The dried precursor was calcined in a tube furnace by raising the temperature to 800 °C at 5 °C / min for 2 h to obtain NiO@CuO material.
[0075] Comparative Example 3
[0076] (1) 2 mmol of Zn(AC) 2Place in a 100 mL beaker and add 25 mL of deionized water. Stir magnetically for 20-30 min. 2 When it is completely dissolved, add 2 mmol of thiourea to form solution C;
[0077] (2) Solution C was magnetically stirred for 20 min, and then placed in a 100 mL stainless steel hydrothermal reactor with a polytetrafluoroethylene liner for hydrothermal reaction at 140 °C for 8 h. After cooling, the hydrothermal product was centrifuged at high speed and washed with deionized water 3 times and anhydrous ethanol 2 times, and finally dried at 60 °C for 12 h to obtain the precursor;
[0078] (3) The dried precursor is calcined in a tube furnace at a temperature of 5 °C / min to 800 °C for 2 h to obtain ZnO material.
[0079] Effect Example
[0080] 1. Sample test characterization
[0081] The NiO@CuO / ZnO composite catalytic material of Example 1, the NiO@CuO material of Comparative Example 2 and the CuO material were subjected to XRD testing, and the obtained XRD diffraction patterns are as follows: Figure 1 As shown. Figure 1 It can be seen that the diffraction peaks corresponding to the NiO@CuO / ZnO sample correspond to the NiO@CuO and CuO crystal planes, respectively, which shows that NiO@CuO / ZnO was successfully prepared.
[0082] 2. Test on degradation of antibiotics in water
[0083] (1) Antibiotic degradation test was performed on the NiO@CuO / ZnO composite catalytic material, NiO material, NiO@CuO material and ZnO material prepared in Example 1 and Comparative Examples 1 to 3.
[0084] Degradation experiment: Use a measuring cylinder to measure 100 mL of 10 mg / L ciprofloxacin solution into a conical flask, and perform the following 7 experiments at the same time, adding the following degradation materials:
[0085] A, no addition, blank group;
[0086] B. 30 mg persulfate (PMS);
[0087] C, 30 mg NiO@CuO / ZnO;
[0088] D, 30 mg NiO@CuO+PMS;
[0089] E, 30 mg NiO+PMS;
[0090] F, 30 mg ZnO+PMS;
[0091] G, 30 mg NiO@CuO / ZnO+PMS.
[0092] Each experimental group was placed on a magnetic stirrer, the speed was adjusted to a certain level, and samples were taken at specific intervals. After sampling, the absorbance was measured using a UV spectrophotometer. The results were as follows: Figure 2 As shown, the degradation rate of ciprofloxacin was calculated by absorbance, degradation rate = (1-C / C 0 )×100%.
[0093] Depend on Figure 2 It can be seen that the blank group and the experimental group with only the addition of NiO@CuO (3:3)-0.2g / ZnO composite catalytic material had almost no degradation effect on ciprofloxacin. In the experimental group with only the addition of PMS, ciprofloxacin was degraded to a certain extent, but the degradation efficiency was very low. In the experimental group with the simultaneous addition of NiO@CuO (3:3)-0.2g / ZnO and PMS, the degradation efficiency of ciprofloxacin was significantly improved. The degradation rate of ciprofloxacin could reach about 75.6% after 90 minutes of degradation, which has a good effect and good stability.
[0094] The materials prepared in Examples 1 to 3 all degraded CIP to a certain extent, but the NiO@CuO (3:3)-0.2g / ZnO prepared in Example 1 had the strongest ability to degrade ciprofloxacin compared with other materials prepared in Example 1. Therefore, adding PMS, NiO@CuO (3:3)-0.2g / ZnO composite catalytic material to activate hydrogen persulfate (PMS) can promote the generation of active free radicals and improve the degradation efficiency of pollutants in water.
[0095] (2) Using the NiO@CuO (3:3)-0.2 g / ZnO prepared in Example 1 and the NiO@CuO / ZnO composite catalytic materials with other molar ratios prepared in Examples 2 and 3 as catalysts, three groups of degradation experiments were set up. First, the three groups of water to be treated were placed in 100 mL conical flasks respectively, 30 mg of catalyst was added to each group of water to be treated, and 30 mg of PMS was added at the same time. The conical flask containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in FIG. Figure 3 shown.
[0096] Depend on Figure 3 It can be seen that the NiO@CuO / ZnO / PMS system has a certain degree of degradation of CIP, among which the NiO@CuO (3:3) / ZnO activated PMS prepared in Example 1 has stronger degradation ability for CIP than the catalysts in the other two groups of degradation experiments.
[0097] (3) Using the composite catalytic materials of Examples 1 and Examples 4 to 6 as catalysts, four groups of degradation experiments were set up. First, the four groups of water to be treated were placed in 100 mL conical flasks respectively. 30 mg of catalyst was added to each group of water to be treated. 30 mg of PMS was added at the same time. The conical flask containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in FIG. Figure 4 shown.
[0098] Depend on Figure 4 It can be seen that the CAT / PMS system has a certain degree of degradation of CIP, among which the NiO@CuO (3:3)-0.2g / ZnO activated PMS prepared in Example 1 has stronger degradation ability for CIP than the catalysts in the other three groups of degradation experiments.
[0099] 3. Experimental analysis of the effect of the amount of NiO@CuO (3:3)-0.2g / ZnO composite catalytic material and PMS on the degradation effect during the degradation process
[0100] (1) The effect of the amount of NiO@CuO (3:3)-0.2g / ZnO composite catalytic material prepared in Example 1 on the degradation efficiency was experimentally studied. 30mg, 40mg, 50mg, and 60mg of NiO@CuO (3:3)-0.2g / ZnO were used as degradation materials, ciprofloxacin solution was used as the solution to be degraded, and 30mg of PMS was added to carry out degradation experiments. After sampling, the absorbance was measured by ultraviolet spectrophotometer. The results are as follows: Figure 5 (a). Figure 5 (a) It can be seen that the amount of NiO@CuO (3:3)-0.2g / ZnO composite catalyst material has a certain influence on the degradation efficiency. The degradation efficiency is best when the amount of NiO@CuO (3:3)-0.2g / ZnO is 50mg, so the catalyst is selected to continue the study. NiO@CuO (3:3)-0.2g / ZnO can catalyze PMS to produce SO4 with strong oxidizing properties. - and •OH react with pollutants and then degrade them into small molecules of CO 2 and H 2 O;
[0101] (2) Using the NiO@CuO (3:3)-0.2g / ZnO composite catalytic material prepared in Example 1 as a catalyst, four groups of degradation experiments with different amounts of PMS added were set up. First, the four groups of water to be treated were placed in 100mL conical flasks, 50 mg of catalyst was added to each group of water to be treated, and 30 mg, 40 mg, 50 mg, and 60 mg of PMS were added at the same time. The conical flask containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in Figure 2. Figure 5 (b). Figure 5 (b) It can be seen that when the catalyst dosage is 50 mg, the degradation rate of CIP in the system with a PMS dosage of 50 mg is the highest, reaching 91.2%.
[0102] 4. Effect of coexisting anions and organic matter in the degradation wastewater on NiO@CuO (3:3)-0.2g / ZnO composite catalytic materials
[0103] Using the NiO@CuO (3:3)-0.2 g / ZnO composite catalytic material prepared in Example 1 as a catalyst, four groups of degradation experiments were set up. First, the four groups of treated water were placed in 100 mL conical flasks, 50 mg of the composite catalytic material was added to each group of treated water, and 50 mg of PMS was added at the same time. Cl was added to each of the four experiments. - 、NO 3 - , HCO 3 - The addition amount of the four substances was set to 1 mmol, 5 mmol, 10 mmol and 15 mmol respectively. The conical flask containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in Figure 6 shown.
[0104] Depend on Figure 6 It can be seen that NO 3 - , Cl - The degradation efficiency of CIP activated by PMS was slightly affected by HA catalysts, while HCO 3 - The degradation capacity of the system has a certain influence, which may be due to HCO 3 - Quenching is caused by a certain amount of active substances.
[0105] 5. Effect of pH value of aqueous solution on NiO@CuO (3:3)-0.2g / ZnO composite catalytic material
[0106] Using the NiO@CuO (3:3)-0.2g / ZnO composite catalytic material prepared in Example 1 as a catalyst, 5 groups of degradation experiments were set up to analyze the pH range of the composite catalytic material for degradation of antibiotic wastewater. First, 5 groups of water to be treated were placed in conical flasks, 50 mg of the composite catalytic material was added to each group of water to be treated, and 50 mg of PMS was added at the same time. The pH value of the CIP solution was adjusted to 3, 5, 7, 9, and 11 with 1M sulfuric acid and sodium hydroxide solution, respectively. The transparent reaction container containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in the figure. Figure 7 shown.
[0107] Depend on Figure 7 It can be seen that when the pH value is 7, the degradation rate of 10 mg / L CIP by NiO@CuO (3:3)-0.2 g / ZnO + PMS system is 91.2% in 180 min, which has the highest degradation efficiency. Secondly, when the pH value is 5, the degradation rate of 10 mg / L CIP by NiO@CuO (3:3)-0.2 g / ZnO + PMS system is 90.8% in 180 min.
[0108] The present invention synthesizes a NiO@CuO (3:3)-0.2g / ZnO composite catalytic material, wherein Ni and Cu produce a good synergistic effect, and the introduction of ZnO enhances the electron mobility and high conductivity of NiO@CuO, accelerates the catalysis of NiO@CuO in PMS activation, and enables the NiO@CuO (3:3)-0.2g / ZnO composite catalytic material to have higher catalytic activity.
[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a NiO@CuO / ZnO composite catalytic material, characterized in that: The method comprises the following steps: (1) Dissolve Ni(NO3)2•6H2O and Cu(NO3)2•3H2O in a mixed solution of deionized water and ethylene glycol to obtain solution A; dissolve thiourea in a mixed solution of deionized water and ethylene glycol to obtain solution B; dissolve Zn(AC)2 in deionized water and add thiourea to obtain solution C; (2) Add solution B dropwise into solution A, stir vigorously, transfer into a high-pressure reactor, and perform a hydrothermal reaction at 160-200°C for 20-28 h. After the reaction is completed, centrifuge the reaction product to separate the hydrothermal product, wash and dry the hydrothermal product in sequence to obtain a precursor; ultrasonically mix the precursor with deionized water to obtain a precursor solution; (3) adding solution C to the precursor solution and conducting a hydrothermal reaction at 120-160° C. for 6-10 h. After the reaction is completed, centrifuging the reaction product to obtain the hydrothermal product, and then drying, grinding, and calcining the hydrothermal product in sequence to obtain a NiO@CuO / ZnO composite catalytic material.
2. The method according to claim 1, characterized in that In step (1), in the solution A, the molar volume ratio of Ni(NO3)2•6H2O, Cu(NO3)2•3H2O, deionized water, and ethylene glycol is 2~4 mmol:2~4 mmol:25 mL:25 mL; In the solution B, the molar volume ratio of thiourea, deionized water and ethylene glycol is 24 mmol:10 mL:10 mL; In the solution C, the molar volume ratio of Zn(AC)2, deionized water, and thiourea is 2 mmol:25 mL:2 mmol.
3. The method according to claim 2, characterized in that In step (2), the molar ratio of Ni(NO3)2•6H2O in solution A to thiourea in solution B is 2~4 mmol:24 mmol.
4. The method according to claim 3, characterized in that In step (3), the mass molar ratio of Zn(AC)2 in the precursor and solution C is 0.1 g~0.3 g:2 mmol.
5. The method according to claim 4, characterized in that The molar mass ratio of Zn(AC)2, Cu(NO3)2•3H2O and precursor is 2 mmol:3 mmol:0.2 g.
6. The method according to claim 1, characterized in that In step (3), the calcination conditions are as follows: calcination temperature 600-1000°C, heating rate 5°C / min, and calcination time 1-3 h.
7. The NiO@CuO / ZnO composite catalytic material prepared by the method according to any one of claims 1 to 6.
8. Use of the NiO@CuO / ZnO composite catalytic material as claimed in claim 7 in activating persulfate to treat wastewater.
9. The use according to claim 8, characterized in that The pollutants in the wastewater are antibiotic pollutants.
10. The use according to claim 8, characterized in that The pH value of the wastewater is 3-11.
Citation Information
Patent Citations
MoS2atCuCo2S4 composite material as well as preparation method and application thereof
CN114425370A
Doped carbonaceous materials for photocatalytic removal of pollutants under visible light, making methods and applications of same
US20190015818A1