Catalyst

By using catalysts composed of non-precious metal catalysts, including alumina and titanium oxide, as well as Ni, Co and Mo, the cost-intensive problems in H2-SCR technology are solved, and efficient reduction of nitrogen oxides is achieved, providing an economical and effective Nitrogen oxide emission reduction scheme.

CN118892843APending Publication Date: 2024-11-05BEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410813587.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-12-06
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The precious metal catalysts used in the existing H2-SCR technology are expensive, and the technology that leads to reduced nitrogen oxide emissions has economic problems.

Method used

A catalyst consisting of 20-80% alumina and 20-80% titanium oxide is used, which contains 0.2-4.5% Ni, 2.5-6.5% Co and 0.5-2.0% Mo. The Ni, Co and Mo content meet the specific relationship. The use of precious metals is avoided in the catalytic reduction process of nitrogen oxides and hydrogen.

Benefits of technology

The catalyst shows good nitrogen oxide reduction activity under room temperature and normal pressure conditions, reducing the cost of H2-SCR technology and providing an economical and effective nitrogen oxide emission reduction solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004907909880000091
    Figure BDA0004907909880000091
Patent Text Reader

Abstract

The invention relates to a catalyst, which comprises a carrier composed of 40-45% of alumina and 55-60% of titanium oxide; the catalyst also comprises the following elements based on 100% of the carrier: 0.9-1.1% of Ni; 4.8% to 5.2% of Co; and from 1.5% to 1.75% Mo; the contents of all the components are calculated by weight; and the contents of Ni, Co and Mo meet the following relational expression: Mo (Co + Ni) / NiCo is greater than or equal to 1.9 and less than or equal to 2.0. The catalyst provided by the invention does not contain noble metal, and has good catalytic activity for NOx reduction; the reduction method based on the catalyst can solve the problem that the H2-selective catalytic reduction technology is high in cost.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the Chinese patent application filed on December 6, 2022, with application number 202211555596.2, and invention name “Catalyst, method for reducing nitrogen oxides and application of catalyst”. Technical Field

[0002] The invention belongs to the technical field of catalysts, and particularly relates to a catalyst. Background Art

[0003] Nitrogen oxides NO x It is one of the main pollutants causing acid rain, photochemical smog and greenhouse effect. According to statistics, NO x About 60% comes from fossil fuels. Therefore, reducing nitrogen oxide emissions is one of the effective means of air pollution control.

[0004] Using the Selective Catalytic Reduction (SCR) method to treat exhaust gas can effectively reduce the emission of nitrogen oxides. Among them, the selective catalytic reduction (H2-SCR) technology using H2 as a reducing agent has the advantages of clean process, no secondary pollution, and good economy. At present, the catalyst used in H2-SCR technology is mainly a precious metal catalyst.

[0005] However, precious metal catalysts use precious metals as raw materials and are expensive, which leads to the high cost of H2-SCR technology. Summary of the invention

[0006] In order to solve the problems in the prior art and provide a new solution for reducing nitrogen oxide emissions, the present invention provides a catalyst comprising

[0007] a carrier composed of 20-80% alumina and 20-80% titania; and

[0008] Taking the carrier as 100%, the following elements are also included:

[0009] 0.2-4.5% Ni;

[0010] 2.5-6.5% Co; and

[0011] 0.5-2.0% Mo;

[0012] And the contents of Ni, Co and Mo satisfy the following relationship:

[0013] 0.3≦Mo(Co+Ni) / NiCo≦4.0.

[0014] At the same time, the present invention also provides a method for reducing NO xMethod, NO x is a substance selected from NO, N2O, NO2, N2O3, N2O4, N2O5 or a mixture thereof, the method comprising making NO x Reaction with H2, characterized in that the reaction is carried out in the presence of the above-mentioned catalyst of the present invention.

[0015] The present invention also provides the use of the above catalyst in reducing NOx, especially in reducing NO.

[0016] The catalyst of the present invention does not contain precious metals and is useful for reducing NO x It has good catalytic activity; the reduction method based on the catalyst can solve the problem of high cost of H2-SCR technology. DETAILED DESCRIPTION

[0017] In the present invention, unless otherwise specified, all component contents are based on weight.

[0018] In the present invention, unless otherwise specified, all operations are carried out at room temperature and normal pressure.

[0019] The present invention provides a catalyst, comprising

[0020] a carrier composed of 20-80% alumina and 20-80% titania; and

[0021] Taking the carrier as 100%, the following elements are also included:

[0022] 0.2-4.5% Ni;

[0023] 2.5-6.5% Co; and

[0024] 0.5-2.0% Mo;

[0025] And the contents of Ni, Co and Mo (based on values ​​excluding %, for example, Ni is calculated as a value between 0.2-4.5, the same below) satisfy the following relationship:

[0026] 0.3≦Mo(Co+Ni) / NiCo≦4.0.

[0027] In a preferred embodiment of the present invention, the catalyst of the present invention comprises

[0028] a carrier composed of 40-45% alumina and 55-60% titania; and

[0029] Taking the carrier as 100%, the following elements are also included:

[0030] 0.9-1.1% Ni;

[0031] 4.8-5.2% Co; and

[0032] 1.5-1.75% Mo;

[0033] And the contents of Ni, Co and Mo satisfy the following relationship:

[0034] 1.9≦Mo(Co+Ni) / NiCo≦2.0.

[0035] In a further preferred embodiment of the present invention, the catalyst of the present invention consists of the following components:

[0036] a carrier composed of 40-45% gamma-alumina and 55-60% titania; and

[0037] Taking the carrier as 100%, the following elements:

[0038] 0.9-1.1% Ni;

[0039] 4.8-5.2% Co; and

[0040] 1.5-1.75% Mo;

[0041] And the contents of Ni, Co and Mo satisfy the following relationship:

[0042] 1.9≦Mo(Co+Ni) / NiCo≦2.0.

[0043] In a further preferred embodiment of the present invention, the catalyst of the present invention consists of the following components:

[0044] a carrier composed of 41-43% gamma-alumina and 57-59% titania; and

[0045] Taking the carrier as 100%, the following elements:

[0046] 0.95-1.05% Ni;

[0047] 4.9-5.1% Co; and

[0048] 1.60-1.65% Mo;

[0049] And the contents of Ni, Co and Mo satisfy the following relationship:

[0050] 1.9≦Mo(Co+Ni) / NiCo≦2.0.

[0051] In the present invention, the carrier is a mixture of titanium oxide TiO2 and aluminum oxide Al2O3, and commercially available titanium oxide and aluminum oxide can be used, preferably in the form of micro-spherical particles. Preferably, the titanium oxide TiO2 has an anatase structure, and the Al2O3 is micro-spherical γ-Al2O3.

[0052] In a preferred embodiment, the weight ratio of the TiO2 and the γ-Al2O3 is TiO2:γ-Al2O3=(1-4):1, preferably (1.2-1.6):1, and more preferably (1.30-1.35):1.

[0053] The catalyst of the present invention can be prepared by a common impregnation method. For example, it can be prepared as follows: an aqueous solution of a metal salt of each active component is mixed with a mixture of carrier titanium oxide and aluminum oxide, and if necessary, heating and stirring are performed; after drying, the temperature is lowered; and then roasting is performed to obtain the catalyst.

[0054] When the aqueous solution of the metal salt of each active component is mixed with the carrier titanium oxide and aluminum oxide, the total volume of the solution and the total volume of the carrier mixture are preferably (1-2.5):1, preferably (1-2):1. Mixing can be carried out at room temperature, or at 20-60°C, preferably at 25-50°C, optionally under heating and stirring conditions, for 0.1-2 hours, preferably 0.2-1.5 hours. Then stand for 2-24 hours, preferably stand for 6-16 hours, more preferably stand for 10-15 hours. The drying temperature is 60-130°C, preferably 65-90°C, and the drying is 1-8 hours, preferably 3.5-6.5 hours. The calcination temperature is 380-650°C, preferably 400-630°C, especially 580-620°C; the calcination time is 1.5-8 hours, preferably 3.5-6.0 hours.

[0055] The metal salt of each active component can be a water-soluble salt of each metal, especially a nitrate of each metal.

[0056] When preparing the catalyst, preferably, the carrier uses the 40-60 mesh portion. Preferably, the prepared catalyst uses the 40-60 mesh portion.

[0057] The present invention reduces NO x In the method, NO x is a substance selected from NO, N2O, NO2, N2O3, N2O4, N2O5 or a mixture thereof, in particular, NO x The method comprises making NO x and reacting with H2, said reaction being carried out in the presence of the catalyst of the present invention.

[0058] In the method of the present invention, the catalyst can be used in a fixed bed manner, and the reaction process can be carried out in a tubular reactor. The product can be detected by any known method, such as using an online chromatograph, a nitrogen and oxygen analyzer, etc.

[0059] In a preferred embodiment of the method of the present invention, the catalyst is reduced at 400-500° C. for 0.5-3 hours, wherein the reducing gas comprises a mixture of H2 and N2, wherein the volume percentage of H2 is 1-20%. Subsequently, NOx is reduced. In a further embodiment, NO x The reaction with H2 is carried out at 270-300°C, in particular at 290-300°C. Preferably, NO x In the reaction with H2, the reaction gas contains H2 / NO x , where the volume ratio is H2 / NO x =1-5, preferably 2-3.5, H2 and NO x It accounts for 0.05-1.5% of the gas volume, preferably 0.1-1.2%, and the rest is inert gas, such as nitrogen, argon, etc. Preferably, the catalyst is a 40-60 mesh catalyst.

[0060] In the present invention, all devices or equipment used may be conventional devices or equipment known in the art, and may be purchased or obtained by methods disclosed in literature.

[0061] It goes without saying that the various catalysts of the present invention described above, i.e., the catalysts in the broadest range and the catalysts in each preferred embodiment, can be used in the method of reducing NOx of the present invention, constituting corresponding wide-range methods and various preferred methods, and combined with the method characteristics of the present invention itself, forming a further preferred method.

[0062] The present invention also provides the use of the above catalyst in reducing NOx, especially in reducing NO.

[0063] Catalytic reduction of NO by using the catalyst of the present invention x , avoiding the use of expensive catalysts containing precious metals and solving the high cost problem of H2-SCR technology.

[0064] The present invention will be described in further detail below in conjunction with embodiments.

[0065] The following examples are only used to explain the present invention, but not to limit the present invention.

[0066] I. Catalyst Preparation Example

[0067] In the following preparation examples, the catalyst was selected from the part between 20-40 mesh.

[0068] Comparative Example 1

[0069] Weigh 44.59g of nickel nitrate (Ni(NO3)2·6H2O, molecular weight 290.80) and 13.12g of cerium nitrate (Ce(NO3)3·6H2O, molecular weight 434.23) and dissolve them in 200mL of water to obtain a first mixed metal salt solution. Then place 100g of carrier TiO2 into the first mixed metal salt solution, stir for 1 hour, and let stand for 4 hours. Then, evaporate the water in vacuum at 70°C with strong stirring to obtain a first catalyst precursor. The first catalyst precursor is calcined at 800°C for 2 hours to obtain a first catalyst.

[0070] Based on 100 g of the carrier mass, the Ni loading of the first catalyst was 9.00% (loading=active component mass / carrier mass, the same below), and the Ce loading was 4.23%.

[0071] Comparative Example 2

[0072] Weigh 29.64 g of cobalt nitrate (Co(NO3)2·6H2O, molecular weight 291.03) and 30.89 g of ammonium heptamolybdate ((NH4)6Mo7O 24 ·4H2O, molecular weight is 1235.86) is dissolved in 200mL water to obtain a second mixed metal salt solution. Then 100g of the second carrier γ-Al2O3 is placed in the second mixed metal salt solution and stirred for 1 hour, and then allowed to stand for 12 hours. Thereafter, the water is evaporated under vacuum at 70°C and under strong stirring to obtain a second catalyst precursor. The second catalyst precursor is calcined at 500°C for 5 hours to obtain a second catalyst.

[0073] Based on the mass of the support, the second catalyst has a Co loading of 6% and a Mo loading of 16.79%.

[0074] Example 3

[0075] Weigh 29.63 g of cobalt nitrate (Co(NO3)2·6H2O), 2.48 g of nickel nitrate (Ni(NO3)2·6H2O), and 3.22 g of ammonium heptamolybdate ((NH4)6Mo7O 24 ·4H2O) was dissolved in 200mL water to obtain a third mixed metal salt solution. Then 100g of the third carrier (including 80g TiO2 and 20g γ-Al2O3) was placed in the third mixed metal salt solution and stirred for 1 hour, and then allowed to stand for 24 hours. Thereafter, the water was evaporated under vacuum at 70°C and under strong stirring to obtain a third catalyst precursor. The third catalyst precursor was calcined at 400°C for 6 hours to obtain a third catalyst.

[0076] Based on the mass of the support, the third catalyst has a Co loading of 6.00%, a Ni loading of 0.5%, and a Mo loading of 1.75%.

[0077] Example 4

[0078] Weigh 14.81 g of cobalt nitrate (Co(NO3)2·6H2O), 19.82 g of nickel nitrate (Ni(NO3)2·6H2O) and 1.20 g of ammonium heptamolybdate ((NH4)6Mo7O 24 ·4H2O) was dissolved in 200mL water to obtain a fourth mixed metal salt solution. Then 100g of the fourth carrier (including 60g TiO2 and 40g γ-Al2O3) was placed in the fourth mixed metal salt solution and stirred for 1 hour, and then allowed to stand for 12 hours. Thereafter, the water was evaporated under vacuum at 70°C and under strong stirring to obtain a fourth catalyst precursor. The fourth catalyst precursor was calcined at 600°C for 4 hours to obtain a fourth catalyst.

[0079] Based on the mass of the support, the fourth catalyst has a Ni loading of 4.00%, a Co loading of 3.00%, and a Mo loading of 0.65%.

[0080] Comparative Example 5

[0081] Weigh 19.82g of nickel nitrate (Ni(NO3)2·6H2O) and 2.75g of iron nitrate

[0082] (Fe(NO3)3·9H2O, molecular weight is 403.85) and 2.94g cerium nitrate (Ce(NO3)3·6H2O) are dissolved in 200mL water to prepare the fifth mixed metal salt solution. Then 100g of the fifth carrier (including 75gTiO2 and 25gγ-Al2O3) is placed in the fifth mixed metal salt solution and stirred for 1 hour, and then allowed to stand for 12 hours. Thereafter, the water is evaporated under vacuum at 70°C and under strong stirring to obtain the fifth catalyst precursor. The fifth catalyst precursor is calcined at 600°C for 4 hours to obtain the fifth catalyst.

[0083] Based on the weight of the support, the fifth catalyst has a Ni loading of 4.00%, a Fe loading of 0.38%, and a Ce loading of 0.95%.

[0084] Example 6

[0085] Weigh 24.70 g of cobalt nitrate (Co(NO3)2·6H2O), 4.96 g of nickel nitrate (Ni(NO3)2·6H2O) and 3.0 g of ammonium heptamolybdate ((NH4)6Mo7O 24·4H2O) was dissolved in 200mL water to obtain a sixth mixed metal salt solution. Then 100g of the sixth carrier (including 57.15g TiO2 and 42.85g γ-Al2O3) was placed in the sixth mixed metal salt solution and stirred for 1 hour, and then allowed to stand for 12 hours. Thereafter, the water was evaporated under vacuum at 70°C and under strong stirring to obtain a sixth catalyst precursor. The sixth catalyst precursor was calcined at 600°C for 4 hours to obtain a sixth catalyst.

[0086] Based on the weight of the support, the sixth catalyst has a Co loading of 5.00%, a Ni loading of 1%, and a Mo loading of 1.63%.

[0087] Comparative Example 7

[0088] Weigh 4.94g of cobalt nitrate (Co(NO3)2·6H2O), 14.86g of nickel nitrate (Ni(NO3)2·6H2O) and 6.87g of iron nitrate (Fe(NO3)3·9H2O) and dissolve them in 200mL of water to obtain the seventh mixed metal salt solution. Then, place 100g of the seventh carrier (including 80g of TiO2 and 20g of γ-Al2O3) into the seventh mixed metal salt solution, stir for 1 hour, and let stand for 12 hours. Thereafter, evaporate the water in a vacuum at 70°C with strong stirring to obtain the seventh catalyst precursor. The seventh catalyst precursor is calcined at 500°C for 5 hours to obtain the seventh catalyst.

[0089] Based on the weight of the support, the seventh catalyst has a Co loading of 1.00%, a Ni loading of 3.00%, and a Fe loading of 0.95%.

[0090] The catalyst compositions of Examples 1-7 are summarized in Table 1.

[0091] Table 1 Catalyst composition (wt.%, γ-Al2O3+TiO2 is 100%)

[0092] Example Comparison 1 Comparison 2 3 4 Contrast 5 6 Contrast 7 <![CDATA[γ-Al2O3]]> 100 20 40 25 42.85 20 <![CDATA[TiO2]]> 100 80 60 75 57.15 80 Ni 9 0.5 4 4 1 3 Co 6 6.0 3 5 1 Mo 16.79 1.75 0.65 1.63 Fe 0.38 0.95 Ce 4.23 0.95 Mo(Ni+Co) / NiCo 3.79 0.379 1.956

[0093] II. Catalyst activity test

[0094] When evaluating the denitration catalytic activity of the catalyst of the present invention, a PJ-05TDC fixed bed reactor system of Beijing Shishi Jiaqi Zhiyuan Technology Development Co., Ltd. was used, in which a quartz tube reactor (inner diameter 8 mm) was used, and the catalyst was filled in the middle of the reactor in the form of a fixed bed, and both ends of the reactor were filled with 40-60 mesh quartz sand.

[0095] 1. Catalyst pre-reduction

[0096] First, the catalyst was pre-reduced, and the total gas flow rate was 50 mL / min. 0.4 g (20-40 mesh) of catalyst was heated (10°C / min) to 450°C in a H2 / Ar (8% H2, volume percentage) gas flow and kept at a constant temperature for 40 min. A gas mass spectrometer was used to measure and record the signal changes of hydrogen. A stable hydrogen signal means that the pre-reduction is complete. After stopping heating and cooling to room temperature, the H2 / Ar mixed gas was switched to Ar gas and purged for 10 min for standby use.

[0097] 2.H2-SCR denitrification reaction

[0098] After the pre-reduction is completed and the temperature is lowered to room temperature, switch to one of the following reaction gases, with a total gas flow rate of 80 mL / min; program the temperature from room temperature to 500°C at a rate of 4°C / min.

[0099] Reaction gas composition (volume percentage):

[0100] Reaction gas 1: 0.06% NO, 0.12% H2, the rest Ar;

[0101] Reaction gas 2: 0.06% NO, 0.12% H2, 0.02% SO2, and the rest Ar.

[0102] A 42i-HL nitrogen oxide analyzer (Thermo Electron, USA) was used to detect the NO concentration in the exhaust gas in real time.

[0103] According to T 50 and T 90 Analysis of the catalytic performance of the denitrification catalyst, T 50 and T 90 They represent the reaction temperatures (°C) corresponding to NO removal rates of 50% and 90%, respectively. The lower the reaction temperature, the better the catalyst activity.

[0104] The results are summarized in Table 2, where the catalyst number corresponds to the example number, and the catalyst specific surface area is measured by nitrogen adsorption method; the columns where SO2=0 and SO2=0.02% correspond to the reaction results of reaction gas 1 and reaction gas 2, respectively.

[0105] Table 2 Catalyst activity test results

[0106]

[0107] As shown in Table 2, the catalysts of Examples 3, 4 and 6 exhibited good catalytic activities.

Claims

1. A catalyst comprising a carrier composed of 40-45% alumina and 55-60% titania; and Taking the carrier as 100%, the following elements are also included: 0.9-1.1% Ni; 4.8-5.2% Co; and 1.5-1.75% Mo; All component contents are by weight; And the contents of Ni, Co and Mo satisfy the following relationship: 1.9≦Mo(Co+Ni) / NiCo≦2.

0.

2. The catalyst according to claim 1, comprising the following components composition: a carrier composed of 40-45% gamma-alumina and 55-60% titania; and Taking the carrier as 100%, the following elements are also included: 0.9-1.1% Ni; 4.8-5.2% Co; and 1.5-1.75% Mo; All component contents are by weight; And the contents of Ni, Co and Mo satisfy the following relationship: 1.9≦Mo(Co+Ni) / NiCo≦2.

0.

3. The catalyst according to claim 2, comprising the following components composition: a carrier composed of 41-43% gamma-alumina and 57-59% titania; and Taking the carrier as 100%, the following elements are also included: 0.95-1.05% Ni; 4.9-5.1% Co; and 1.60-1.65% Mo; All component contents are by weight; And the contents of Ni, Co and Mo satisfy the following relationship: 1.9≦Mo(Co+Ni) / NiCo≦2.0.

Citation Information

Patent Citations

  • Catalyst with meso pore characteristics and application thereof

    CN102240570A

  • Catalyst for selective catalytic reduction denitration of steam electric plant and preparation method thereof

    CN103055888A