Catalyst for catalyzing oxidation of 5-hydroxymethylfurfural to prepare FDCA as well as preparation method and application of catalyst
By calcining soluble metal salts containing Mn, Co, Ni, Cu, Fe and Ce with organic substances containing hydroxyl or carboxyl groups, a catalyst with lattice defects and oxygen vacancies was prepared, which solved the high cost of existing catalysts and FDCA yield. The problem of low efficiency of FDCA preparation is achieved.
Patent Information
- Application Number
- CN202410784841.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-06-18
AI Technical Summary
The existing catalysts used for the catalytic oxidation of 5-hydroxymethylfurfural are high in cost, complex preparation process and low FDCA yield, making it difficult to promote in industrial applications.
The soluble metal salt containing Mn, Co, Ni, Cu, Fe and Ce is mixed and calcined with the hydroxyl or carboxyl group-containing organic matter, and a metal oxide catalyst with lattice defects and oxygen vacancies are obtained by high temperature calcining of 300°C to 400°C. , improve the catalytic effect.
It achieves a catalytic effect with low cost, simple preparation process and high FDCA yield, and is suitable for industrial applications.
Smart Images

Figure CN118892844A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomass chemical industry, and particularly relates to a catalyst for preparing FDCA from 5-hydroxymethylfurfural, and a preparation method and application thereof. Background Art
[0002] As environmental, energy and climate issues become increasingly prominent, carbon emission reduction has become a focus of the world's attention. Bio-based chemicals can be produced by biomass conversion, which has significant carbon reduction benefits from a life cycle perspective. 2,5-Furandicarboxylic acid (FDCA) is one of the most promising bio-based chemicals with broad application prospects.
[0003] At present, the methods for synthesizing 2,5-furandicarboxylic acid (FDCA) using 5-hydroxymethylfurfural (HMF) as raw material mainly include biosynthesis, photocatalytic oxidation, electrocatalytic oxidation and chemical catalytic oxidation. Among them, chemical catalytic oxidation is the earliest developed and most mature method, including homogeneous catalytic system and heterogeneous catalytic system.
[0004] Heterogeneous catalytic systems mainly include two types: precious metal catalysts and non-precious metal catalysts. The precious metal catalysts used for the catalytic oxidation of HMF to prepare FDCA are mainly based on four precious metals: gold, platinum, palladium, and ruthenium. They all have very good catalytic performance (FDCA yields of 95%-99%), and the conditions are mild, and can even be catalytically oxidized under alkaline conditions. However, the cost of using precious metal catalysts is too expensive and difficult to promote in industrial applications.
[0005] Non-precious metal catalysts are mainly based on transition metals, such as manganese, cobalt, nickel, etc. Although many non-precious metal catalysts reported so far have good catalytic effects, their preparation processes are complicated and difficult to carry out large-scale industrial production, and the yield of FDCA is low. Summary of the invention
[0006] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, one object of the present invention is to provide a catalyst for preparing FDCA from 5-hydroxymethylfurfural, and a preparation method and application thereof, wherein the catalyst has low cost, simple preparation process, excellent catalytic effect, and high FDCA yield.
[0007] The first aspect of the present invention provides a method for preparing a catalyst for catalyzing the oxidation of 5-hydroxymethylfurfural to prepare FDCA, comprising: mixing and calcining an organic matter containing a hydroxyl group or a carboxyl group with a soluble metal salt; the soluble metal salt contains at least two of Mn, Co, Ni, Cu, Fe and Ce; and the calcination temperature is 300°C-400°C.
[0008] The inventors found that by mixing and calcining a soluble metal salt (containing at least two of Mn, Co, Ni, Cu, Fe and Ce) with an organic matter containing a hydroxyl group or a carboxyl group, the soluble metal salt reacts with the organic matter containing a hydroxyl group or a carboxyl group during the mixing process to obtain an insoluble metal salt, and then calcining at a high temperature of 300°C-400°C to obtain a metal oxide with lattice defects and more oxygen vacancies. When the calcination temperature is lower than 300°C, it is impossible to obtain a metal oxide crystal form that is conducive to catalytic oxidation of HMF to generate FDCA, and the obtained solid material does not really begin to decompose at this temperature, so it is not conducive to catalytic oxidation. When the temperature is higher than 400°C, the crystal form of the catalyst obtained after calcination changes. Although it can still catalytically oxidize HMF, the effect is significantly reduced. Therefore, a metal oxide with lattice defects and more oxygen vacancies can be obtained by calcining at a high temperature of 300°C-400°C. The crystal form of the metal oxide is spinel MnCo2O4.5, which has more lattice defects and oxygen vacancies, and can improve the catalytic effect of oxygen oxidation of HMF to generate FDCA. In addition, the catalyst is prepared by using at least two soluble metal salts, and the catalyst of at least two metals has a larger specific surface area and pore size, and is more conducive to electron transfer, improves the catalyst oxygen mobility, and is more likely to produce lattice oxygen and oxygen vacancies. The d orbital electronic structure of the transition metal gives it good catalytic activity, can provide effective electron transfer, and promote the activation of oxygen molecules to achieve a good molecular oxygen activation efficiency and catalytic HMF oxidation conversion effect. Thus, a catalyst with low cost, simple preparation process, excellent catalytic effect, and high FDCA yield is obtained.
[0009] In addition, the method for preparing a catalyst for preparing FDCA from 5-hydroxymethylfurfural according to the present invention also has the following technical features:
[0010] In some embodiments of the present invention, the organic matter containing hydroxyl or carboxyl groups includes at least one of glucose, fructose, citric acid, lactic acid, tartaric acid, malonic acid, succinic acid and oxalic acid. By adding organic matter, it is beneficial to form insoluble metal salts, and regulate oxygen vacancies and lattice oxygen structures, thereby improving the performance of the catalyst.
[0011] In some embodiments of the present invention, the organic matter containing hydroxyl or carboxyl groups includes succinic acid or oxalic acid, thereby further improving the performance of the catalyst.
[0012] In some embodiments of the present invention, the soluble metal salt includes at least one of nitrate, acetate and sulfate. Thus, a catalyst with excellent catalytic effect and high FDCA yield is obtained.
[0013] In some embodiments of the present invention, the soluble metal salt contains Mn and Co. Thus, a better catalytic effect is obtained, and the HMF conversion rate and FDCA yield are improved.
[0014] In some embodiments of the present invention, the molar ratio of Mn to Co is 1-10:1-10. Thus, a better catalytic effect is further obtained, and the HMF conversion rate and FDCA yield are further improved.
[0015] In some embodiments of the present invention, the molar ratio of the organic matter containing hydroxyl or carboxyl groups to the soluble metal salt is 1-10:1-10. This is conducive to further forming insoluble metal salts, and regulating oxygen vacancies and lattice oxygen structures, thereby further improving the performance of the catalyst.
[0016] In some embodiments of the present invention, the mixing conditions include: a mixing time of 6 hours to 24 hours; and / or a mixing temperature of 25° C. to 40° C. Thus, a uniformly mixed insoluble metal salt with uniform particle size can be formed.
[0017] In some embodiments of the present invention, the calcination time is 1 h to 6 h, thereby forming a metal oxide with catalytic activity, which in turn activates molecular oxygen to catalyze the oxidation of HMF to generate FDCA.
[0018] The second aspect of the present invention provides a catalyst for preparing FDCA from 5-hydroxymethylfurfural, wherein the catalyst comprises a catalyst prepared by any one of the methods described above. Thus, the catalyst has low cost, simple preparation process, excellent catalytic effect, and high FDCA yield.
[0019] The third aspect of the present invention provides a method for preparing FDCA from 5-hydroxymethylfurfural, comprising: mixing 5-hydroxymethylfurfural with a catalyst to prepare FDCA, wherein the catalyst comprises a catalyst prepared by any one of the methods described above or the catalyst described above. Thus, the method has a simple preparation process, a high HMF conversion rate, and a high FDCA yield.
[0020] In some embodiments of the present invention, the method comprises: (1) mixing 5-hydroxymethylfurfural, an inorganic base, an oxidant and a catalyst to react to obtain a reaction mixture; (2) performing solid-liquid separation on the reaction mixture to obtain a solid substance and a filtrate; (3) treating the filtrate to obtain an FDCA product. Thus, the method for preparing FDCA from 5-hydroxymethylfurfural has a simple preparation process, a high HMF conversion rate, and a high FDCA yield.
[0021] In addition, the method for preparing FDCA from 5-hydroxymethylfurfural of the present invention also has the following technical features:
[0022] In some embodiments of the present invention, in the method for preparing FDCA from 5-hydroxymethylfurfural, in step (1), the concentration of 5-hydroxymethylfurfural is 0.1 mol / L-2 mol / L. Thus, the method for preparing FDCA from 5-hydroxymethylfurfural has a high HMF conversion rate and a high FDCA yield.
[0023] In some embodiments of the present invention, in the method for preparing FDCA from 5-hydroxymethylfurfural, in step (1), the inorganic base contains at least one of sodium carbonate, potassium carbonate, sodium bicarbonate and potassium bicarbonate. Thus, the method for preparing FDCA from 5-hydroxymethylfurfural has a high HMF conversion rate and a high FDCA yield.
[0024] In some embodiments of the present invention, in the method for preparing FDCA from 5-hydroxymethylfurfural, in step (1), the concentration of the inorganic base is 0.001 mol / L-4 mol / L, thereby obtaining a higher FDCA yield.
[0025] In some embodiments of the present invention, in the method for preparing FDCA from 5-hydroxymethylfurfural, in step (1), the oxidant is air or oxygen, the reaction pressure is 0.1MPa-5MPa; and / or the reaction temperature is 20°C-170°C; and / or the reaction time is 1h-10h. Thus, a higher FDCA yield can be obtained.
[0026] In some embodiments of the present invention, in the method for preparing FDCA from 5-hydroxymethylfurfural, in step (1), the mass ratio of 5-hydroxymethylfurfural to catalyst is 1-10:1-10. Thus, the method has excellent catalytic effect, high HMF conversion rate, and high FDCA yield.
[0027] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0029] Figure 1 The present invention is a schematic flow diagram of a method for preparing a catalyst for preparing FDCA from 5-hydroxymethylfurfural according to an embodiment of the present invention.
[0030] Figure 2 The present invention is a schematic flow diagram of a method for preparing FDCA from 5-hydroxymethylfurfural according to an embodiment of the present invention.
[0031] Reference numerals: 1 - mixer; 2 - calciner; 3 - oxidation reactor; 4 - separation purifier. DETAILED DESCRIPTION
[0032] The embodiments of the present invention are described in detail below, which are intended to explain the present invention but should not be construed as limiting the present invention.
[0033] The first aspect of the present invention provides a method for preparing a catalyst for preparing FDCA from 5-hydroxymethylfurfural, comprising: mixing and calcining an organic matter containing a hydroxyl group or a carboxyl group with a soluble metal salt; the soluble metal salt contains at least two of Mn, Co, Ni, Cu, Fe and Ce; and the calcination temperature is 300°C-400°C.
[0034] The inventors found that by mixing and calcining a soluble metal salt (containing at least two of Mn, Co, Ni, Cu, Fe and Ce) with an organic matter containing a hydroxyl group or a carboxyl group, the soluble metal salt reacts with the organic matter containing a hydroxyl group or a carboxyl group during the mixing process to obtain an insoluble metal salt, and then calcining at a high temperature of 300°C-400°C to obtain a metal oxide with lattice defects and more oxygen vacancies. When the calcination temperature is lower than 300°C, it is impossible to obtain a metal oxide crystal form that is conducive to catalytic oxidation of HMF to generate FDCA, and the obtained solid material does not really begin to decompose at this temperature, so it is not conducive to catalytic oxidation. When the temperature is higher than 400°C, the crystal form of the catalyst obtained after calcination changes. Although it can still catalytically oxidize HMF, the effect is significantly reduced. Therefore, a metal oxide with lattice defects and more oxygen vacancies can be obtained by calcining at a high temperature of 300°C-400°C. The crystal form of the metal oxide is spinel MnCo2O4.5, which has more lattice defects and oxygen vacancies, and can improve the catalytic effect of oxygen oxidation of HMF to generate FDCA. In addition, the catalyst is prepared by using at least two soluble metal salts, and the catalyst of at least two metals has a larger specific surface area and pore size, and is more conducive to electron transfer, improves the catalyst oxygen mobility, and is more likely to produce lattice oxygen and oxygen vacancies. The d orbital electronic structure of the transition metal gives it good catalytic activity, can provide effective electron transfer, and promote the activation of oxygen molecules to achieve a good molecular oxygen activation efficiency and catalytic HMF oxidation conversion effect. Thus, a catalyst with low cost, simple preparation process, excellent catalytic effect, and high FDCA yield is obtained.
[0035] According to an embodiment of the present invention, the mixing of the organic matter containing hydroxyl or carboxyl groups and the soluble metal salt is carried out under the condition of solvent assistance. The solvent includes at least one of water, methanol and ethanol. By using a solvent, the organic matter containing hydroxyl or carboxyl groups and the soluble metal salt can be better dispersed, thereby forming a more uniform mixture and a precipitate with a more uniform particle size, thereby improving the performance of the catalyst.
[0036] It should be noted that there is no particular limitation on the method for mixing the organic matter containing hydroxyl or carboxyl groups with the soluble metal salt described in the present invention, as long as a uniform mixture and a precipitate with uniform particle size can be formed, and those skilled in the art can make a selection according to actual needs.
[0037] For example, in some embodiments of the present invention, the metal salt and the organic matter are mixed by respectively dissolving the organic matter containing hydroxyl or carboxyl groups and the soluble metal salt in a solvent and then adding them by drops.
[0038] For example, in some embodiments of the present invention, metal salts and organic matter are dissolved in a solvent and then continuously mixed through a microchannel reactor to form a uniform mixture and a precipitate with uniform particle size.
[0039] In some embodiments of the present invention, the calcination is performed after filtering and drying the solid matter produced after mixing.
[0040] It should be noted that the method of filtering and drying the solid matter before calcination described in the present invention is a conventional technical means in the art, and those skilled in the art can select it according to actual needs.
[0041] In some embodiments of the present invention, the organic matter containing hydroxyl or carboxyl groups includes at least one of glucose, fructose, citric acid, lactic acid, tartaric acid, malonic acid, succinic acid and oxalic acid. By adding organic matter, the pore structure properties such as the specific surface area and total pore volume of the catalyst can be improved, and the reduction of some metal oxides during the calcination process can be promoted to form abundant low-valent metal ions, thereby promoting the formation of more oxygen vacancies, promoting the catalytic oxidation of HMF, and improving the reaction activity.
[0042] In some embodiments of the present invention, the organic matter containing hydroxyl or carboxyl groups includes succinic acid or oxalic acid, thereby further improving the performance of the catalyst.
[0043] In some embodiments of the present invention, the soluble metal salt includes at least one of nitrate, acetate and sulfate. Thus, a catalyst with excellent catalytic effect and high FDCA yield is obtained.
[0044] In some embodiments of the present invention, the soluble metal salt contains Mn and Co. On the one hand, both manganese and cobalt belong to transition metals, and their d orbital electronic structure makes them have good catalytic activity, can provide effective electron transfer, and promote the activation of oxygen molecules to achieve good molecular oxygen activation efficiency and catalytic HMF oxidation conversion effect; on the other hand, the synergistic effect of manganese and cobalt makes it easier to adsorb substrates and oxidants, and at the same time, abundant oxygen vacancies and lattice oxygen are formed, which promotes the adsorption and activation process of HMF and oxidants, and then the catalytic oxidation of HMF can be carried out efficiently. In some embodiments of the present invention, the molar ratio of Mn and Co is 1-10:1-10. For example, the molar ratio of Mn and Co can be 1:1, 1:5, 1:10, 10:1, 10:5, etc. Therefore, by controlling the molar ratio of Mn and Co within this range, the oxygen mobility of the corresponding catalyst can be affected, and a better catalytic effect can be further obtained, and the HMF conversion rate and FDCA yield can be further improved.
[0045] In some embodiments of the present invention, the molar ratio of the organic matter containing hydroxyl or carboxyl groups to the soluble metal salt is 1-10:1-10, for example, 1:1, 1:5, 1:10, 10:1, 10:5, etc. This is conducive to further regulating oxygen vacancies and lattice oxygen structures, thereby further improving the performance of the catalyst.
[0046] In some embodiments of the present invention, the mixing conditions include: a mixing time of 6 hours to 24 hours; and / or a mixing temperature of 25° C. to 40° C. For example, the mixing time may be 6 hours, 10 hours, 14 hours, 18 hours, 24 hours, etc. For example, the mixing temperature may be 25° C., 30° C., 35° C., 40° C., etc. Thus, a uniformly mixed insoluble metal salt with uniform particle size can be formed.
[0047] In some embodiments of the present invention, the calcination time is 1 h-6 h. For example, the calcination time can be 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, etc. Thus, a metal oxide with catalytic activity is formed, and then the molecular oxygen is activated to catalyze the oxidation of HMF to generate FDCA.
[0048] The second aspect of the present invention provides a catalyst for preparing FDCA from 5-hydroxymethylfurfural, wherein the catalyst comprises a catalyst prepared by any one of the methods described above. Thus, the catalyst has low cost, simple preparation process, excellent catalytic effect, and high FDCA yield.
[0049] The third aspect of the present invention provides a method for preparing FDCA from 5-hydroxymethylfurfural, comprising: mixing 5-hydroxymethylfurfural with a catalyst to prepare FDCA, wherein the catalyst comprises the catalyst prepared by the method described in the first aspect above or the catalyst described in the second aspect above. Thus, the method has a simple preparation process, a high HMF conversion rate, and a high FDCA yield.
[0050] In some embodiments of the present invention, the method for preparing FDCA from 5-hydroxymethylfurfural is as follows: Figure 1 ,include:
[0051] S100: Mix 5-hydroxymethylfurfural, inorganic base, oxidant and catalyst for reaction
[0052] In this step, 5-hydroxymethylfurfural, an inorganic base, an oxidant and a catalyst are mixed and reacted. Under the action of the catalyst, 5-hydroxymethylfurfural is oxidized by the oxidant, and intermediate products 5-hydroxymethyl-2-furancarboxylic acid and 5-formyl-2-furancarboxylic acid are formed in the process, and finally the product 2,5-furandicarboxylic acid is formed.
[0053] In some embodiments of the present invention, in S100, the concentration of 5-hydroxymethylfurfural is 0.1 mol / L-2 mol / L. For example, the concentration of 5-hydroxymethylfurfural can be 0.1 mol / L, 0.5 mol / L, 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, etc. Thus, the method for preparing FDCA from 5-hydroxymethylfurfural has high HMF conversion rate and high FDCA yield.
[0054] In some embodiments of the present invention, in S100, the inorganic base contains at least one of sodium carbonate, potassium carbonate, sodium bicarbonate and potassium bicarbonate. Thus, the method for preparing FDCA from 5-hydroxymethylfurfural has a high HMF conversion rate and a high FDCA yield.
[0055] In some embodiments of the present invention, in S100, the concentration of the inorganic base is 0.001mol / L-4mol / L. For example, the concentration of the inorganic base can be 0.001mol / L, 0.01mol / L, 0.05mol / L, 0.1mol / L, 0.5mol / L, 1.0mol / L, 2.0mol / L, 3.0mol / L, 4.0mol / L, etc. Thus, a higher FDCA yield can be obtained.
[0056] In some embodiments of the present invention, in S100, the oxidant is air or oxygen, the reaction pressure is 0.1MPa-5MPa; and / or the reaction temperature is 20°C-170°C; and / or the reaction time is 1h-10h. Increasing the pressure of air or oxygen is conducive to the oxidation reaction, thereby, within the operating parameter range provided by the present invention, a higher FDCA yield can be obtained.
[0057] In some embodiments of the present invention, in S100, the mass ratio of 5-hydroxymethylfurfural to the catalyst is 1-10:1-10. For example, the mass ratio of 5-hydroxymethylfurfural to the catalyst can be 1:1, 1:5, 1:10, 10:1, 10:5, etc. Thus, the method has excellent catalytic effect, high HMF conversion rate, and high FDCA yield.
[0058] S200: Solid-liquid separation of the reaction mixture
[0059] In this step, the reaction mixture is subjected to solid-liquid separation to obtain a solid substance and a filtrate.
[0060] S300: Treat the filtrate
[0061] In this step, the filtrate is treated to obtain the FDCA product. Specifically, the filtrate is treated by decolorization, acidification, filtration, washing and recrystallization. It should be noted that the decolorization, acidification, filtration, washing and recrystallization of the filtrate described in the present invention are conventional technical means in the art, and those skilled in the art can select according to actual needs.
[0062] Therefore, the method for preparing FDCA from 5-hydroxymethylfurfural has a simple preparation process, a high HMF conversion rate, and a high FDCA yield.
[0063] One embodiment of the present invention is, with reference to the attached Figure 2 Soluble metal salts and organic matter containing hydroxyl or carboxyl groups are added to a mixer 1, and the obtained solid mixture is calcined in a calciner 2 to obtain a catalyst. In an oxidation reactor 3, 5-hydroxymethylfurfural, an inorganic base, an oxidant and a catalyst are mixed and reacted, and FDCA is obtained through a separation purifier 4.
[0064] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0065] Preparation Example
[0066] The invention is used to illustrate the preparation method of the catalyst for preparing FDCA from 5-hydroxymethylfurfural according to the present invention.
[0067] Preparation Example 1
[0068] 2 mmol of manganese nitrate, 8 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to ethanol, mixed and placed for 24 hours, and the obtained solid mixture was calcined at 300°C for 3 hours to obtain a catalyst denoted as Mn-Co, wherein the molar ratio of manganese to cobalt was 0.25:1, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0069] Preparation Example 2
[0070] Preparation Example 2 was carried out in the same manner as Preparation Example 1, except that 7.5 mmol of oxalic acid in Preparation Example 1 was replaced by 7.5 mmol of tartaric acid, 7.5 mmol of malonic acid, and 7.5 mmol of succinic acid, respectively, and the obtained catalysts were recorded as Mn / Co-1, Mn / Co-2, and Mn / Co-3, respectively. The molar ratio of manganese to cobalt was 0.25:1, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0071] Preparation Example 3
[0072] Preparation Example 3 was carried out in the same manner as Preparation Example 1, except that the molar ratio of manganese to cobalt in Preparation Example 1 was changed to 3:7, 4:6, 5:5, and 6:4, respectively. The molar ratio of oxalic acid to metal salt was 0.75:1, and the obtained catalysts were recorded as Mn-Co-37, Mn-Co-46, Mn-Co-55, and Mn-Co-64, respectively.
[0073] Preparation Example 4
[0074] 4 mmol of manganese nitrate, 6 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, mixed and placed for 24 hours, and then the obtained solid mixture was calcined at 300°C for 2 hours to obtain a catalyst named Mn-Co-300, wherein the molar ratio of manganese to cobalt was 4:6, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0075] 4 mmol of manganese nitrate, 6 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, mixed and placed for 24 hours, and then the solid mixture was calcined at 400°C for 2 hours to obtain a catalyst named Mn-Co-400, wherein the molar ratio of manganese to cobalt was 4:6, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0076] Preparation Example 5
[0077] 4 mmol of manganese nitrate, 6 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, mixed and placed for 24 hours, and then the solid mixture was calcined at 300°C for 2 hours to obtain a catalyst named Mn-Co-0.75, wherein the molar ratio of manganese to cobalt was 4:6, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0078] Based on the preparation method of catalyst Mn-Co-0.75, the difference is that 7.5mmol oxalic acid in Mn-Co-0.75 is replaced by 3mmol oxalic acid, 5mmol oxalic acid, 10mmol oxalic acid, and 20mmol oxalic acid, respectively, and the obtained catalysts are recorded as Mn-Co-0.3, Mn-Co-0.5, Mn-Co-1.0, and Mn-Co-2.0, respectively. Among them, the molar ratio of manganese to cobalt is 4:6, and the molar ratio of oxalic acid to metal salt is 0.3:1, 0.5:1, 1.0:1, and 2.0:1, respectively.
[0079] Preparation Example 6
[0080] Preparation Example 6 was carried out in the same manner as Preparation Example 1, except that the manganese nitrate and cobalt nitrate in Preparation Example 1 were replaced by manganese nitrate and nickel nitrate, manganese nitrate and iron nitrate, manganese nitrate and cerium nitrate, copper nitrate and cobalt nitrate, and manganese nitrate and cobalt nitrate, respectively, and the obtained catalysts were recorded as Mn-Ni, Mn-Fe, Mn-Ce, Cu-Co, and Mn-Co, respectively. Among them, the molar ratio of Mn-Ni, Mn-Fe, Mn-Ce, Cu-Co, and Mn-Co was 0.25:1, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0081] Example
[0082] The invention is used to illustrate the method for preparing FDCA from 5-hydroxymethylfurfural using the catalyst of the present invention.
[0083] In the following examples, the HMF conversion rate and the FDCA yield were calculated by the following formulas:
[0084] HMF conversion rate (%) = (1-HMF molar amount in product / HMF initial molar amount) × 100%
[0085] FDCA yield (%) = (FDCA molar amount in product / HMF initial molar amount) × 100%
[0086] Example 1
[0087] 1mmol 5-hydroxymethylfurfural, 2mmol sodium bicarbonate and 20ml water were added to a 70ml autoclave, 100mg Mn-Co catalyst was added and the autoclave was sealed, 1.6MPa oxygen was introduced, and the mixture was heated to 140°C at a stirring rate of 500rpm and maintained for 8h. After the reaction was completed, the mixture was cooled to room temperature and sampled for testing. It was found that the Mn-Co catalyst had a 100% HMF conversion rate and a 89.06% FDCA yield.
[0088] Example 2
[0089] Example 2 was carried out in the same manner as Example 1, except that the 100 mg Mn-Co catalyst in Example 1 was replaced with 100 mg Mn-Co-1, 100 mg Mn-Co-2, and 100 mg Mn-Co-3, respectively. After the reaction was completed, the reaction was cooled to room temperature and samples were taken for testing. The results are listed in Table 1. It can be seen that the catalyst containing Mn-Co and oxalic acid has a HMF conversion rate of 100% and a FDCA yield of 84.73%.
[0090] Table 1 Test results of catalysts with different organic matter added
[0091] catalyst HMF conversion rate (%) FDCA yield (%) Mn-Co-1 100.00 53.05 Mn-Co-2 100.00 56.98 Mn-Co-3 100.00 84.73
[0092] Example 3
[0093] Example 3 was carried out in the same manner as Example 1, except that the Mn-Co catalyst in Example 1 was replaced by Mn-Co-37, Mn-Co-46, Mn-Co-55 and Mn-Co-64, respectively, and the results are shown in Table 2. It can be seen that the catalyst containing Mn-Co and oxalic acid, and when the molar ratio of Mn-Co is 4:6, has a HMF conversion rate of 100% and a FDCA yield of 92.78%.
[0094] Table 2 Effect of different manganese-cobalt molar ratios on the catalytic performance of the catalyst
[0095]
[0096]
[0097] Example 4
[0098] 1mmol 5-hydroxymethylfurfural, 2mmol sodium bicarbonate and 20ml water were added to a 70ml high-pressure reactor, 150mg Mn-Co-300 catalyst was added and the reactor was sealed, 1.6MPa oxygen was introduced, and the mixture was heated to 140°C at a stirring rate of 500rpm and maintained for 4h. After the reaction was completed, the mixture was cooled to room temperature and samples were taken for detection. The results are shown in Table 3.
[0099] 1 mmol 5-hydroxymethylfurfural, 2 mmol sodium bicarbonate and 20 ml water were added to a 70 ml high-pressure reactor, 150 mg Mn-Co-400 catalyst was added and the reactor was sealed, 1.6 MPa oxygen was introduced, and the mixture was heated to 140 ° C at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The results are shown in Table 3.
[0100] It can be seen that the catalyst containing Mn-Co and oxalic acid, with a Mn-Co molar ratio of 4:6 and a catalyst calcined at a temperature of 300° C., has a HMF conversion rate of 100% and a FDCA yield of 92.89%.
[0101] Table 3 Effect of different calcination temperatures on the catalytic performance of the catalyst
[0102] catalyst HMF conversion rate (%) FDCA yield (%) Mn-Co-300 100.00 92.89 Mn-Co-400 100.00 69.21
[0103] Example 5
[0104] Example 5 was carried out based on the reaction method of Mn-Co-300 in Example 3, except that the Mn-Co-300 catalyst in Example 3 was replaced by Mn-Co-0.3, Mn-Co-0.5, Mn-Co-0.75, Mn-Co-1.0, and Mn-Co-2.0, respectively, and the results are shown in Table 4. It can be seen that the catalyst containing Mn-Co and oxalic acid, wherein the molar ratio of Mn-Co is 4:6, the calcination temperature of the catalyst is 300°C, and the molar ratio of oxalic acid to Mn-Co metal salt is 0.75:1, has a HMF conversion rate of 100% and a FDCA yield of 92.72%.
[0105] Table 4 Effect of different oxalic acid addition amounts on the catalytic performance of the catalyst
[0106] catalyst HMF conversion rate (%) FDCA yield (%) Mn-Co-0.3 98.91 51.31 Mn-Co-0.5 100.00 59.11 Mn-Co-0.75 100.00 92.72 Mn-Co-1.0 100.00 92.26 Mn-Co-2.0 100.00 89.18
[0107] Example 6
[0108] Example 6 was carried out in the same manner as Example 1, except that the Mn-Co catalyst in Example 1 was replaced by Mn-Ni, Mn-Fe, Mn-Ce, and Cu-Co, respectively. After the reaction was completed, the catalyst was cooled to room temperature and samples were taken for testing. The results are listed in Table 5.
[0109] Table 5 Comparison of the effects of different catalysts on HMF oxidation conversion
[0110] catalyst HMF conversion rate (%) FDCA yield (%) Mn-Ni 67.36 61.46 Mn-Fe 85.34 58.61 Mn-Ce 93.30 79.87 Cu-Co 85.02 56.77
[0111] Example 7
[0112] 1 mmol 5-hydroxymethylfurfural and 20 ml water were added to a 70 ml high-pressure reactor, followed by 1 mmol potassium carbonate and 150 mg Mn-Co-46 catalyst. The reactor was sealed, 1.6 MPa oxygen was introduced, and the reactor was heated to 140°C at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, the reactor was cooled to room temperature and samples were taken for testing. The results are listed in Table 6.
[0113] 1 mmol 5-hydroxymethylfurfural and 20 ml water were added to a 70 ml high-pressure reactor, followed by 1 mmol sodium carbonate and 150 mg Mn-Co-46 catalyst. The reactor was sealed, 1.6 MPa oxygen was introduced, and the reactor was heated to 140°C at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, the reactor was cooled to room temperature and samples were taken for testing. The results are listed in Table 6.
[0114] 1 mmol 5-hydroxymethylfurfural and 20 ml water were added to a 70 ml high-pressure reactor, followed by 2 mmol potassium bicarbonate and 150 mg Mn-Co-46 catalyst. The reactor was sealed, 1.6 MPa oxygen was introduced, and the reactor was heated to 140°C at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, the reactor was cooled to room temperature and samples were taken for testing. The results are listed in Table 6.
[0115] It can be seen that the catalyst containing Mn-Co and oxalic acid, wherein the molar ratio of Mn-Co is 4:6, and the inorganic base is potassium bicarbonate, has a HMF conversion rate of 100% and a FDCA yield of 93.42%.
[0116] Table 6 Effect of different inorganic bases on the oxidation of HMF to FDCA
[0117] catalyst Inorganic base HMF conversion rate (%) FDCA yield (%) Mn-Co-46 Potassium carbonate 100.00 87.94 Mn-Co-46 Sodium carbonate 100.00 88.73 Mn-Co-46 Potassium bicarbonate 100.00 93.42 Mn-Co-46 Sodium bicarbonate 100.00 92.89
[0118] Example 8
[0119] 1 mmol 5-hydroxymethylfurfural, 2 mmol sodium bicarbonate and 20 ml water were added to a 70 ml high-pressure reactor, and 150 mg Mn-Co-46 catalyst was added. The reactor was sealed, and 1.6 MPa of oxygen was introduced. The reactor was heated to 140 ° C at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The results are shown in Table 7.
[0120] 1.5 mmol 5-hydroxymethylfurfural, 3 mmol sodium bicarbonate and 20 ml water were added to a 70 ml high-pressure reactor, and 150 mg Mn-Co-46 catalyst was added. The reactor was sealed, and 1.6 MPa of oxygen was introduced. The reactor was heated to 140 ° C at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The results are shown in Table 7.
[0121] 2mmol 5-hydroxymethylfurfural, 4mmol sodium bicarbonate and 20ml water were added to a 70ml high-pressure reactor, and 150mg Mn-Co-46 catalyst was added. The reactor was sealed, 1.6MPa oxygen was introduced, and the mixture was heated to 140°C at a stirring rate of 500rpm and maintained for 4h. After the reaction was completed, the mixture was cooled to room temperature and sampled for detection. The results are shown in Table 7.
[0122] Table 7 Effect of HMF concentration on FDCA yield
[0123]
[0124] Example 9
[0125] 2 mmol of manganese nitrate, 4 mmol of cerium nitrate, 4 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, and the solid mixture was mixed and placed for 24 hours. The catalyst obtained after calcination at 300° C. for 3 hours was recorded as Mn-Ce-Co.
[0126] 1mmol 5-hydroxymethylfurfural, 2mmol sodium bicarbonate and 20ml water were added to a 70ml high-pressure reactor, and 100mg Mn-Ce-Co catalyst was added. The reactor was sealed, 1.6MPa oxygen was introduced, and it was heated to 140°C at a stirring rate of 500rpm and maintained for 8h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The obtained Mn-Ce-Co catalyst had a HMF conversion rate of 100% and a FDCA yield of 70.0%.
[0127] Comparative Example 1
[0128] 4 mmol of manganese nitrate, 6 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, mixed and placed for 24 hours, and then the obtained solid mixture was calcined at 200° C. for 2 hours to obtain a catalyst, which was recorded as Mn-Co-200. Among them, the molar ratio of manganese to cobalt was 4:6, and the molar ratio of oxalic acid to metal salt was 0.75:1.
[0129] 1 mmol 5-hydroxymethylfurfural, 2 mmol sodium bicarbonate and 20 ml water were added to a 70 ml high-pressure reactor, 150 mg Mn-Co-200 catalyst was added, the reactor was sealed, 1.6 MPa oxygen was introduced, and it was heated to 140°C at a stirring rate of 500 rpm and maintained for 4 hours. After the reaction was completed, it was cooled to room temperature and sampled for detection. The Mn / Co-200 catalyst had only a HMF conversion rate of 38.76% and a FDCA yield of 1.45%.
[0130] Comparative Example 2
[0131] Comparative Example 2 was carried out in the same manner as Comparative Example 1, except that the solid mixture was calcined at 500° C. for 2 h to obtain a catalyst, which was recorded as Mn-Co-500. After sampling and testing, although the Mn / Co-500 catalyst had a 100% HMF conversion rate, it had only a 1.45% FDCA yield.
[0132] Comparative Example 3
[0133] 4 mmol of manganese nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, and the mixture was allowed to stand for 24 hours. The obtained solid mixture was calcined at 300° C. for 2 hours. The obtained catalyst was recorded as Mn-300.
[0134] 1mmol 5-hydroxymethylfurfural, 2mmol sodium bicarbonate and 20ml water were added to a 70ml high-pressure reactor, and 150mg Mn-300 catalyst was added. The reactor was sealed, and 1.6MPa oxygen was introduced. The reactor was heated to 140°C at a stirring rate of 500rpm and maintained for 4h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The HMF conversion rate of the Mn-300 catalyst was 95%, and the FDCA yield was 25%.
[0135] Comparative Example 4
[0136] 6 mmol of cobalt nitrate and 7.5 mmol of oxalic acid were added to 20 ml of ethanol, mixed and allowed to stand for 24 hours, and then the obtained solid mixture was calcined at 300° C. for 2 hours to obtain the catalyst Co-300.
[0137] 1mmol 5-hydroxymethylfurfural, 2mmol sodium bicarbonate and 20ml water were added to a 70ml high-pressure reactor, and 150mg Co-300 catalyst was added. The reactor was sealed, and 1.6MPa oxygen was introduced. The reactor was heated to 140°C at a stirring rate of 500rpm and maintained for 4h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The HMF conversion rate of the Co-300 catalyst was 97%, and the FDCA yield was 5%.
[0138] Comparative Example 5
[0139] 4 mmol of manganese nitrate, 6 mmol of cobalt nitrate and 7.5 mmol of thiourea were added into 20 ml of ethanol, wherein the organic matter was thiourea. After the mixture was allowed to stand for 24 hours, the obtained solid mixture was calcined at 300° C. for 2 hours to obtain a catalyst.
[0140] 1 mmol 5-hydroxymethylfurfural, 2 mmol sodium bicarbonate and 20 ml water were added to a 70 ml high-pressure reactor, and 150 mg of the catalyst prepared as above was added. The reactor was sealed, and 1.6 MPa of oxygen was introduced. The reactor was heated to 140° C. at a stirring rate of 500 rpm and maintained for 4 h. After the reaction was completed, it was cooled to room temperature and sampled for detection. The final HMF conversion rate was 60%, and the FDCA yield was only 3%.
[0141] It can be seen from the data of the above examples and comparative examples that the catalyst of the present invention is used to catalyze the oxidation of 5-hydroxymethylfurfural to prepare FDCA, has excellent catalytic performance and a high FDCA yield, and the preparation method of the catalyst of the present invention is simple and low-cost, and has prospects for industrial application.
[0142] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0143] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a catalyst for catalyzing the oxidation of 5-hydroxymethylfurfural to prepare FDCA, characterized in that: include: The organic matter containing hydroxyl or carboxyl groups is mixed with a soluble metal salt and calcined; The soluble metal salt contains at least two of Mn, Co, Ni, Cu, Fe and Ce; The calcination temperature is 300°C-400°C.
2. The method according to claim 1, characterized in that The organic matter containing hydroxyl or carboxyl groups includes at least one of glucose, fructose, citric acid, lactic acid, tartaric acid, malonic acid, succinic acid and oxalic acid; Succinic acid or oxalic acid is preferred.
3. The method according to claim 1, characterized in that The soluble metal salt includes at least one of nitrate, acetate and sulfate.
4. The method according to claim 1 or 3, characterized in that: The soluble metal salt contains Mn and Co; Optionally, the molar ratio of Mn to Co is 1-10:1-10.
5. The method according to claim 1, characterized in that The molar ratio of the organic matter containing hydroxyl or carboxyl group to the soluble metal salt is 3:(1-10).
6. The method according to claim 1, characterized in that The mixing conditions include: a mixing time of 6 hours to 24 hours; and / or a mixing temperature of 25° C. to 40° C.; Optionally, the calcination time is 1 h-6 h.
7. A catalyst for preparing FDCA from 5-hydroxymethylfurfural, characterized in that: The catalyst comprises a catalyst prepared by any one of claims 1 to 6.
8. A method for preparing FDCA from 5-hydroxymethylfurfural, characterized in that: include: FDCA is prepared by mixing 5-hydroxymethylfurfural with a catalyst, wherein the catalyst comprises a catalyst prepared by any one of claims 1 to 6 or a catalyst according to claim 7.
9. The method according to claim 8, characterized in that include: (1) mixing 5-hydroxymethylfurfural, an inorganic base, an oxidant and a catalyst to react to obtain a reaction mixture; (2) subjecting the reaction mixture to solid-liquid separation to obtain a solid substance and a filtrate; (3) Treat the filtrate to obtain the FDCA product.
10. The method according to claim 9, characterized in that In step (1), the concentration of 5-hydroxymethylfurfural is 0.1 mol / L-2 mol / L; Optionally, in step (1), the inorganic base contains at least one of sodium carbonate, potassium carbonate, sodium bicarbonate and potassium bicarbonate; Optionally, in step (1), the concentration of the inorganic base is 0.001 mol / L-4 mol / L; Optionally, in step (1), the oxidant is air or oxygen, the reaction pressure is 0.1 MPa-5 MPa; and / or, the reaction temperature is 20° C.-170° C.; and / or, the reaction time is 1 h-10 h; Optionally, in step (1), the mass ratio of 5-hydroxymethylfurfural to catalyst is 1-10:1-10.
Citation Information
Patent Citations
Bimetallic oxide catalyst and preparation and using methods thereof
CN112138679A
Double-transition metal hierarchical pore catalyst as well as preparation method and application thereof
CN112569965A
Preparation method of 2,5-furandicarboxylic acid under mild condition
CN112830916A
Bimetal oxide catalyst as well as preparation and use methods thereof
CN113797934A
Preparation method of 2, 5-furandicarboxylic acid
CN115073404A
Cited By
Method for preparing 2, 5-furandicarboxylic acid through selective catalytic oxidation of 5-hydroxymethylfurfural by using nano-microstructured multi-metal oxide
CN119455977A