CdS / Cs3Bi2Br9 heterojunction composite photocatalyst capable of degrading tetracycline hydrochloride and synthesis method of CdS / Cs3Bi2Br9 heterojunction composite photocatalyst
By preparing a CdS/Cs3Bi2Br9 heterojunction photocatalyst, the problems of low activity and poor stability of Cs3Bi2X9 material were solved, and the photocatalytic activity and stability were improved, making it suitable for the degradation of tetracycline hydrochloride.
Patent Information
- Application Number
- CN202410927309.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
Existing Cs3Bi2X9 materials have low photocatalytic activity and poor stability, while lead-based perovskite materials have toxicity issues.
A heterojunction photocatalyst was prepared by in-situ growth of CdS/Cs3Bi2Br9 heterojunctions via supersaturated recrystallization to improve the separation efficiency of photogenerated carriers and increase the stability of the material.
The photocatalytic activity of Cs3Bi2Br9 material was improved, the carrier separation efficiency was increased, and the stability was enhanced, making it suitable for photocatalytic degradation of tetracycline hydrochloride.
Smart Images

Figure CN118892852A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photocatalytic material synthesis technology and application, and specifically relates to a method for preparing a CdS / Cs3Bi2Br9 composite material, and the role of the photocatalyst prepared by the method in the degradation of tetracycline hydrochloride. Background Art
[0002] Faced with the dual challenges of energy shortage and environmental pollution, vigorously developing renewable energy and energy-saving and environmentally friendly new energy has become the basic choice of the energy strategy of countries around the world in the 21st century. Inorganic lead halide perovskite materials have attracted great attention from researchers around the world due to their incredible optoelectronic properties, such as high photoluminescence quantum yield, full visible light spectrum emission, adjustable band gap, high extinction coefficient, low exciton binding energy and excellent charge transport performance. Combined with these special properties, halide perovskite materials have also received widespread attention in the field of photocatalysis.
[0003] Although lead halide perovskite materials have such outstanding optical properties, the toxicity of lead elements and the instability of perovskite quantum dots themselves have become two major obstacles to the development of this material in the field of photocatalysis. In order to solve these problems, the main technical routes are divided into the following two types: one is to use inorganic substances or polymers to encapsulate quantum dots to form a composite structure, so that the quantum dots are isolated from the external environment and the stability is improved; the other is to explore new non-lead perovskite materials, such as using relatively less toxic tin (Sn), bismuth (Bi) or antimony (Sb) elements to replace the lead position, fundamentally getting rid of the "lead dependence" of inorganic lead halide perovskites. Among the many non-lead perovskite materials, the all-inorganic bismuth-based perovskite (Cs3Bi2X9) system has a series of good properties: low toxicity, lone pair s electrons, low dimensionality, good stability, etc. These good properties make Cs3Bi2X9 materials a relatively promising photocatalytic material. However, the problem of low photocatalytic activity and poor stability of Cs3Bi2X9 materials still exists. Summary of the invention
[0004] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and provide a method for preparing and applying a CdS / Cs3Bi2Br9 heterojunction composite photocatalyst. The CdS / Cs3Bi2Br9 heterojunction is grown in situ by a supersaturated recrystallization method. The prepared heterojunction can improve the photocatalytic activity of the Cs3Bi2Br9 material, increase the efficient separation of photogenerated carriers, and increase the stability in water. The specific scheme for implementing the present invention includes the following steps:
[0005] Step 1: Synthesis of CdS
[0006] Weigh cadmium acetate and thiourea in a beaker, add water to the beaker, and stir for 2 hours. Then transfer the solution in the beaker to a reactor, heat to 150 degrees Celsius, and keep warm for 10 hours. Then wash with deionized water 2-3 times, dry in a vacuum oven at 80 degrees Celsius for 12 hours, and collect the final powder.
[0007] Step 2: Weigh 0.425 g of CsBr and 0.6 g of BiBr3 (molar ratio of 2:1), put them in a clean beaker, add 30 ml of dimethyl sulfoxide to fully dissolve them, and record them as solution A1; add 50 ml of ethanol as solvent in another clean beaker, add 0.03 g of CdS prepared in step 1, heat to 80 degrees Celsius, stir and keep warm for 1-2 hours, stir with a magnetic stirrer, and stir at a speed of 1000 rpm, record them as solution A2; slowly add solution A1 dropwise to solution A2, light yellow crystals precipitate, stir for 1-2 hours to end the reaction;
[0008] Step 3: Centrifugal washing to recover solid powder
[0009] Specifically, the centrifuge speed is 6000 rpm, the centrifugation time is 10 minutes, the toluene: methyl acetate is 1:1 and washed 2-4 times, and finally placed in a vacuum drying oven, the drying temperature is 60 degrees Celsius, and the drying time is 12 hours. The CdS / Cs3Bi2Br9 heterojunction photocatalyst is obtained.
[0010] CdS / Cs3Bi2Br9 heterojunction photocatalyst can catalytically degrade tetracycline hydrochloride under irradiation of 300W xenon lamp.
[0011] Specifically, the catalyst is placed in tetracycline hydrochloride wastewater with a concentration of 10 mg / L, mixed evenly, adsorbed in the dark for 60 minutes, and after reaching adsorption equilibrium, a low-power white light xenon lamp is turned on for 60 minutes; wherein the catalyst mass: wastewater volume ratio is 5-100 mg: 50-100 ml.
[0012] Compared with the prior art, the present invention has the following advantages
[0013] The present invention synthesizes lead-free Cs3Bi2Br9 nanocrystals without lead elements, thereby solving the toxicity of lead-based perovskite materials, and the shell CdS can protect the Cs3Bi2Br9 nanocrystals, thereby increasing the stability of the material and the separation efficiency of carriers, and has the characteristics of simple preparation process and low cost. Finally, the composite material is used for photocatalytic degradation of tetracycline hydrochloride, and has broad application prospects in the field of photocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 X-ray crystal diffraction patterns of CdS, Cs3Bi2Br9, and CdS / Cs3Bi2Br9;
[0015] Figure 2 Transmission electron micrographs of CdS, Cs3Bi2Br9, and CdS / Cs3Bi2Br9;
[0016] Figure 3 It is the degradation performance diagram of CdS, Cs3Bi2Br9, and CdS / Cs3Bi2Br9 composite material; DETAILED DESCRIPTION
[0017] The present invention will be further described and illustrated below in conjunction with the embodiments of the present invention.
[0018] Example 1
[0019] The synthesis method of CdS is to weigh cadmium acetate and thiourea in a beaker, add water to the beaker, and stir for 2 hours. Then transfer the solution in the beaker to a reactor, heat it to 150 degrees Celsius, and keep it warm for 10 hours. Then use deionized water to wash 2-3 times, dry it in a vacuum oven at 80 degrees Celsius for 12 hours, collect the final powder, and obtain CdS powder.
[0020] Example 2
[0021] (1) The synthesis method of Cs3Bi2Br9 is as follows: weigh 0.425g of CsBr and 0.6g of BiBr3, place them in a clean beaker, add 30ml of dimethyl sulfoxide to fully dissolve them, and record it as solution A1; add 50ml of ethanol as a solvent in another clean beaker, heat to 80 degrees Celsius, stir and keep warm for 2 hours, stir with a magnetic stirrer, and stir at a speed of 1000rpm, and record it as solution A2; slowly add solution A1 dropwise to solution A2, and light yellow Cs3Bi2Br9 crystals precipitate, and stir for 2 hours to complete the reaction;
[0022] (2) The centrifuge speed is 6000 rpm, the centrifugation time is 10 min, and the mixture is washed 2-4 times with toluene:methyl acetate 1:1, and finally placed in a vacuum drying oven at a drying temperature of 60 degrees Celsius for 12 hours to obtain pure Cs3Bi2Br9 crystals.
[0023] Example 3
[0024] (1) The in-situ synthesis method of CdS / Cs3Bi2Br9 is as follows: weigh 0.425 g of CsBr and 0.6 g of BiBr3, place them in a clean beaker, add 30 ml of dimethyl sulfoxide to fully dissolve them, and record it as solution A1; add 50 ml of ethanol as a solvent in another clean beaker, add 0.03 g of CdS prepared in step 1, heat to 80 degrees Celsius, stir and keep warm for 2 hours, stir with a magnetic stirrer, and stir at a speed of 1000 rpm, and record it as solution A2; slowly add solution A1 dropwise to solution A2, and light yellow crystals precipitate, and stir for 2 hours to complete the reaction;
[0025] (2) The centrifuge speed is 6000 rpm, the centrifugation time is 10 min, and the mixture is washed 2-4 times with toluene:methyl acetate 1:1, and finally placed in a vacuum drying oven at a drying temperature of 60 degrees Celsius for 12 hours to obtain the CdS / Cs3Bi2Br9 heterojunction photocatalyst.
[0026] Example 4
[0027] Weigh 10 mg of the catalyst and a solution of tetracycline hydrochloride with a concentration of 10 mg / L, respectively, and place the solution in a 250 ml photocatalytic reactor. Then, adsorb in the dark for 60 minutes. After reaching adsorption equilibrium, turn on the light source, which is a 300W xenon lamp, for 60 minutes. Take 3 mL of sample every 10 minutes with a pipette, filter the catalyst with a 0.22 μm organic filter, and use a liquid ultraviolet spectrophotometer to detect the change in absorbance at 357 nm for the remaining liquid. Calculate the photodegradation efficiency based on the test results.
[0028] Figure 1 The XRD patterns of pure phase CdS, Cs3Bi2Br9 and CdS / Cs3Bi2Br9 materials synthesized in Examples 1, 2 and 3 show that CdS and Cs3Bi2Br9 have good crystallinity, strong diffraction intensity and completely correspond to the simulated diffraction peaks, indicating that CdS and Cs3Bi2Br9 materials have been successfully synthesized. The XRD pattern of the CdS / Cs3Bi2Br9 composite material shows that the diffraction peaks of the composite material match well with the XRD spectrum of the simulated standard card, indicating that the structure of CdS has not changed during the growth process of Cs3Bi2Br9.
[0029] Figure 2The TEM spectra of (a) pure phase CdS, (b) Cs3Bi2Br9 and (c) CdS / Cs3Bi2Br9 materials synthesized in Examples 1, 2 and 3 show that CdS is in the form of nanospheres and Cs3Bi2Br9 is in the form of hexahedrons. The TEM spectra of CdS / Cs3Bi2Br9 show that a layer of spherical CdS is wrapped on the surface of Cs3Bi2Br9, indicating that the CdS / Cs3Bi2Br9 heterojunction has been successfully synthesized.
[0030] Figure 3 The pure phase CdS, Cs3Bi2Br9 and CdS / Cs3Bi2Br9 materials synthesized in Examples 1, 2 and 3 are applied to the degradation of tetracycline hydrochloride. It can be seen that the degradation efficiency of pure phase CdS is 21% in 60 minutes, that of Cs3Bi2Br9 is 29%, and that of CdS / Cs3Bi2Br9 material is 60%, which is 3 times that of CdS and 2 times that of Cs3Bi2Br9. It has a significant enhancement effect.
[0031] The above analysis shows that the composite degree of CdS / Cs3Bi2Br9 heterojunction photocatalyst using the technical solution of the present invention is good. Moreover, CdS / Cs3Bi2Br9 heterojunction photocatalyst has a good performance in photocatalytic degradation of tetracycline hydrochloride and is a very promising photocatalyst.
Claims
1. An in-situ generated perovskite CdS / Cs 3 Bi 2 Br 9 Heterojunction photocatalysts, It is characterized in that The preparation method comprises the following steps: Step 1: Synthesis of CdS Weigh cadmium acetate and thiourea in a beaker, add water to the beaker, stir for 2 hours, then transfer the solution in the beaker to a reactor, heat to 150 degrees Celsius, and keep warm for 10 hours; Step 2: Weigh CsBr and BiBr 3 The molar ratio is 2:1, placed in a clean beaker, 10-50 ml of dimethyl sulfoxide is added to fully dissolve and recorded as solution A1; 50-100 ml of ethanol is added to another clean beaker as a solvent, and the CdS prepared in step 1 is added, heated to 80 degrees Celsius, stirred and kept warm for 1-2 hours, and the stirring method is stirring with a magnetic stirrer, and the stirring speed is 1000-2000 rpm and recorded as solution A2; Solution A1 is slowly added dropwise to solution A2, and light yellow crystals are precipitated, and the reaction is completed by stirring for 1-2 hours; Step 3: Centrifugal washing to recover solid powder Specifically, the centrifuge speed is 6000-8000rpm, the centrifugation time is 10-20min, toluene: methyl acetate is 1:1, washed 2-4 times, and finally placed in a vacuum drying oven, the drying temperature is 60-80 degrees Celsius, the time is 12 hours, and the CdS / Cs 3 Bi 2 Br 9 Heterojunction photocatalysts.
2. CdS / Cs prepared according to the method of claim 1 3 Bi 2 Br 9 Heterojunction photocatalysts.
3. The in-situ generated perovskite CdS / Cs according to claim 1 3 Bi 2 Br 9 Heterojunction photocatalysts, Features The solution added to beaker A2 is ethanol.
4. The in-situ generated perovskite CdS / Cs according to claim 1 3 Bi 2 Br 9 Heterojunction photocatalysts, Features A2 beaker needs to be heated to 80 degrees Celsius.
5. The in-situ generated perovskite CdS / Cs according to claim 1 3 Bi 2 Br 9 Heterojunction photocatalysts, Features The added CdS is Cs 3 Bi 2 Br 9 10-100% of quality.
6. The CdS / Cs according to claim 2 3 Bi 2 Br 9 Application of heterojunction photocatalyst in photocatalytic degradation of tetracycline hydrochloride.
7. The use according to claim 6, It is characterized in that Specifically include: The catalyst is placed in tetracycline hydrochloride wastewater with a concentration of 5-20 mg / L, mixed evenly, adsorbed in the dark for 30-60 minutes, and after reaching adsorption equilibrium, a low-power white light xenon lamp is turned on for 60 minutes; wherein the catalyst mass: wastewater volume ratio is 5-100 mg: 50-100 ml.
Citation Information
Patent Citations
Bi3O4Cl / CdS composite material and preparation method and application
CN107890877A
Preparation method of magnetic photocatalysis nano-reactor for selectively degrading tetracycline and application of magnetic photocatalysis nano-reactor
CN109174194A
BiOI / CdS composite photocatalyst as well as preparation method and application thereof
CN113398954A
Method for preparing nickel-based metal-organic framework / bismuth oxychloride composite for degrading tetracycline
GB202319977D0