Method for recycling polyester cotton blended fabric

The depolymerization reaction in the alcohol solution was carried out through the composite catalyst system, which solved the problem of difficult separation of polyester and degradation of cotton components in the recycling of polyester cotton blended fabrics, and achieved complete separation and recycling of polyester and cotton fibers, which improved the Recovery and performance promote the recycling of resources.

CN118893071APending Publication Date: 2024-11-05QINGDAO AMINO MATERIAL TECH CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410959184.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Prior Art In the recycling process of polyester cotton blended fabrics, it is difficult to completely separate polyester and the performance of cotton components is degraded, resulting in waste of resources and secondary pollution problems.

Method used

The composite catalyst system is adopted, including the main catalyst being morpholine compounds, the auxiliary catalyst is zwitterionic compounds and di[2-(N,N-dimethylaminoethyl)] ether, and the polypolytic reaction is achieved through the alcohol solution. Complete separation and recovery of ester and cotton fibers.

Benefits of technology

Under mild conditions, the complete depolymerization of polyester and non-destructive retention of cotton fibers are achieved, the mechanical properties and chemical stability of cotton fibers are improved, the recovery rate of polyester depolymerized monomers is improved, and the closed loop of fiber components is achieved recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893071A_ABST
    Figure CN118893071A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recovering a polyester cotton blended fabric, which comprises the following steps: S1, washing the polyester cotton blended fabric by using a mixed solution of alcohol and ester, and then carrying out depolymerization reaction in an alcohol solution by using a composite catalyst to obtain cotton fibers and slurry; the composite catalyst comprises a main catalyst and an auxiliary catalyst; the main catalyst is a morpholine compound, and the auxiliary catalyst is a mixture of a zwitterionic compound and bis [2-(N, N-dimethylaminoethyl)] ether; s2, washing cotton fibers with alcohol to obtain a cleaning solution, mixing the cleaning solution with the slurry, and performing solid-liquid separation to obtain polyester monomers and filtrate; through the depolymerization reaction of the composite catalyst in the solvent and the mutual promotion and synergism of the main catalyst and the auxiliary catalyst, the temperature-sensitive cotton component is kept in a lossless manner, the mechanical property and chemical stability of the cotton component are not influenced, meanwhile, the complete separation of the polyester and the cotton fiber can be realized, the polyester is completely depolymerized, and the recovery rate of the polyester monomer is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to a method for recycling polyester-cotton blended fabrics. Background Art

[0002] Polyester and cotton blended fabrics are widely used. However, the common method of disposing of polyester-cotton blended fabrics as old clothes is landfill or incineration, which not only wastes a lot of resources but also causes serious secondary pollution.

[0003] To prevent secondary pollution, related technologies have been used to recycle polyester-cotton blended fabrics, but there are problems such as difficulty in completely separating polyester and decreased performance of the recycled cotton component.

[0004] Therefore, it is necessary to provide a recycling solution for polyester-cotton blended fabrics, which can improve the depolymerization rate of polyester while ensuring the performance of the recycled cotton component. Summary of the invention

[0005] In view of this, the present application provides a method for recycling polyester-cotton blended fabrics, which is used to solve the problem of how to improve the separation effect of polyester-cotton blended fabrics and ensure the performance of the recycled cotton component.

[0006] In order to achieve the above technical objectives, this application adopts the following technical solutions:

[0007] In a first aspect, the present application provides a method for recycling polyester-cotton blended fabrics, comprising the following steps:

[0008] S1. After washing the polyester-cotton blended fabric with a mixture of alcohol and ester, depolymerization reaction is carried out in an alcohol solution using a composite catalyst to obtain cotton fiber and slurry; the composite catalyst includes a main catalyst and an auxiliary catalyst; the main catalyst is a morpholine compound, and the auxiliary catalyst is a mixture of a zwitterionic compound and di[2-(N,N-dimethylaminoethyl)] ether;

[0009] S2. Wash the cotton fiber with alcohol to obtain a washing liquid, mix the washing liquid with the slurry, separate the solid and the liquid, and obtain polyester monomers and a filtrate.

[0010] Preferably, the morpholine compound includes one or more of morpholine, N-ethylmorpholine, N-methylmorpholine, morpholinoacetonitrile, N-(2-cyanoethyl)morpholine, morpholine-2-carboxylate, 2-morpholinopyridine, and bismorpholinodiethyl ether.

[0011] Preferably, the zwitterionic compound includes one or more of carboxylic acid betaine, sulfobetaine, and phosphate betaine.

[0012] Preferably, the carboxylate betaine includes dodecyl dimethyl betaine, the sulfo betaine includes dodecyl sulfopropyl betaine, and the phosphate betaine includes dodecyl hydroxypropyl phosphate betaine.

[0013] Preferably, the temperature of the depolymerization reaction is 40-90° C., and the time of the depolymerization reaction is 2-6 hours.

[0014] Preferably, the amount of the composite catalyst is 0.1-20% of the mass of the polyester-cotton blended fabric; the mass ratio of the main catalyst to the auxiliary catalyst is 1:1-10, and the mass ratio of di[2-(N,N-dimethylaminoethyl)]ether to the zwitterionic compound is 1:0.1-10.

[0015] Preferably, in step S1, the alcohol includes methanol, and the ester includes fatty alcohol phosphate; and the washing temperature is 50-70°C.

[0016] Preferably, the cotton content in the polyester-cotton blended fabric is 5-95%.

[0017] Preferably, the method further comprises subjecting the filtrate to atmospheric distillation to recover alcohol, and then subjecting the filtrate to vacuum distillation or extraction to recover the diol monomer of the polyester, as well as the morpholine compound and di[2-(N,N-dimethylaminoethyl)]ether.

[0018] In a second aspect, the present application provides a recycled cotton fiber and polyester depolymerization monomer.

[0019] The beneficial effects of this application are as follows:

[0020] The present application uses a depolymerization reaction of a composite catalyst in a solvent, and through the mutual promotion and synergy of a main catalyst and an auxiliary catalyst, the temperature-sensitive cotton component can be retained intact, and the mechanical properties and chemical stability of the cotton component are not affected. At the same time, the polyester and cotton fibers can be completely separated, the polyester is completely depolymerized, and the recovery rate of the polyester monomer is high. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the polyester monomer dimethyl terephthalate (DMT) recovered after depolymerization provided in Example 6 of the present invention ( 1 H NMR);

[0022] Figure 2 This is the separated and recycled polyester and cotton blended fabric provided in Example 6 of the present invention. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0024] The present application provides a method for recycling polyester-cotton blended fabrics, comprising the following steps:

[0025] S1. After washing the polyester-cotton blended fabric with a mixture of alcohol and ester, depolymerization reaction is carried out in an alcohol solution using a composite catalyst to obtain cotton fiber and slurry; the composite catalyst includes a main catalyst and an auxiliary catalyst; the main catalyst is a morpholine compound, and the auxiliary catalyst is a mixture of a zwitterionic compound and di[2-(N,N-dimethylaminoethyl)] ether;

[0026] S2. Wash the cotton fiber with alcohol to obtain a washing liquid, mix the washing liquid with the slurry, separate the solid and the liquid, and obtain polyester monomers and a filtrate.

[0027] The present invention adopts a composite catalyst system to achieve complete depolymerization of polyester under mild conditions. In the composite catalyst system adopted, morpholine compounds are used as main catalysts to catalyze methanol decomposition of polyester; di[2-(N,N-dimethylaminoethyl)]ether can stabilize the organic base main catalyst cation formed in the catalytic process on the one hand, improve the activity of the main catalyst, and on the other hand, can also be used as an organic base to catalyze methanol decomposition of polyester to a certain extent; zwitterionic compounds can weaken the molecular chain interaction between polyester fiber and cotton component, and the cost is low, further ensuring that the morpholine main catalyst can effectively catalyze methanol, decompose polyester, and ensure complete depolymerization of polyester. The alkalinity of the composite catalyst of the present application is moderate, and the reaction temperature is low, which can make the temperature-sensitive cotton component intactly retained, and the cotton component finally obtained has high fineness, high toughness, and high fiber elongation.

[0028] In some embodiments, the morpholine compound includes one or more of morpholine, N-ethylmorpholine, N-methylmorpholine, morpholinoacetonitrile, N-(2-cyanoethyl)morpholine, morpholine-2-carboxylate, 2-morpholinopyridine, and bismorpholinodiethyl ether.

[0029] In some embodiments, the zwitterionic compound includes one or more of carboxylic acid betaine, sulfobetaine, and phosphobetaine.

[0030] In some embodiments, the carboxylate betaine includes dodecyl dimethyl betaine, the sulfobetaine includes dodecyl sulfopropyl betaine, and the phosphate betaine includes dodecyl hydroxypropyl phosphate betaine.

[0031] In some embodiments, the temperature of the depolymerization reaction is 40-90° C., and the time of the depolymerization reaction is 2-6 hours.

[0032] In some embodiments, the amount of the composite catalyst is 0.1-20% of the mass of the polyester-cotton blended fabric, the mass ratio of the main catalyst to the auxiliary catalyst is 1:1-10, and the mass ratio of di[2-(N,N-dimethylaminoethyl)]ether to the zwitterionic compound is 1:0.1-10. In the above ratios, if the amount is too low, the polyester will be incompletely depolymerized, and if it is too high, the economic efficiency will be reduced, and the cotton component will also be damaged to a certain extent.

[0033] In some embodiments, in step S1, the alcohol includes methanol, and the ester includes fatty alcohol phosphate; the fatty alcohol phosphate includes but is not limited to cetostearyl phosphate, and the washing temperature is 50-70°C. This component is mainly beneficial to the decolorization of the fabric.

[0034] In some embodiments, the cotton content in the polyester-cotton blended fabric is 5-95%.

[0035] In some embodiments, the filtrate is further subjected to atmospheric distillation to recover alcohol, and then subjected to vacuum distillation or extraction to recover the diol monomer of the polyester, as well as morpholine compounds and di[2-(N,N-dimethylaminoethyl)] ether.

[0036] The catalyst system used in the present invention can achieve 100% depolymerization of polyester under low temperature conditions. The depolymerized polyester component can be easily separated from other components, thereby achieving complete separation of polyester and cotton components in polyester / cotton blended fabrics. Moreover, the reaction separation process in the present invention is gentle and efficient, and the cotton fiber can obtain 100% pure components and its fibers are almost not damaged, and can be directly spun into silk threads or used as raw materials to produce regenerated cotton fibers. The recovered polyester depolymerization monomers can also be used for the synthesis of new polyesters, thereby achieving closed-loop recycling of two fiber components in polyester / cotton blended waste, which is of great significance for protecting the ecological environment and reducing the cost of regenerated fibers. In the separation process of the present invention, an organic alkaline catalyst is used to catalyze the breakage of polyester ester bonds. In order to improve the catalytic activity and efficiency of the organic base under low temperature conditions, two auxiliary catalysts are added in the system process, achieving 100% depolymerization reaction of polyester under low temperature conditions, and after adding the auxiliary catalysts, the recovery rate of polyester monomers is significantly improved.

[0037] In a second aspect, the present application provides a recycled cotton fiber and polyester depolymerization monomer.

[0038] In this application, polyester depolymerization refers to the depolymerization of polyester into monomers, thereby falling off and separating from blended fabrics, and then realizing the separation and recovery of polyester components. The polyester in this technology is a polymer containing ester chemical bonds, such as polyethylene terephthalate (PET), polytrimethylene terephthalate (PTT), polybutylene terephthalate (PBT), polyethylene 2,5-furandicarboxylate (PEF), polytrimethylene 2,5-furandicarboxylate (PTF), polybutylene 2,5-furandicarboxylate (PBF), polylactic acid (PLA), polyhydroxyalkanoic acid (PHA), polybutylene glycol succinate (PBS), low melting point polyester copolymer; cotton fiber includes fibers spun from cotton and regenerated cellulose; polyester depolymerization polyester monomers include DMT.

[0039] The present application provides cotton fibers and polyester depolymerization monomers obtained by a recycling method.

[0040] The catalyst system used in the present invention can achieve 100% depolymerization of polyester under low temperature conditions, and at the same time achieve complete separation of polyester and cotton components in polyester-cotton blended fabrics, with a high recovery rate. Moreover, the reaction separation process in the present invention is gentle and efficient, and cotton fibers can obtain 100% pure components and the fibers are almost not damaged, and can be directly spun into silk threads or used as raw materials to produce regenerated cotton fibers. The recovered polyester depolymerization monomers can also be used for the synthesis of new polyesters, thereby realizing the closed-loop recycling of the two fiber components in the polyester-cotton blended waste.

[0041] The present solution is further described below through specific embodiments.

[0042] Source of raw materials:

[0043] The polyester-cotton blended fabric used in the embodiment of the present application is a blended fabric of PET and cotton, wherein the PET content is 55wt%, the cotton content is 45wt%, and the fabric is cut into a 4cm*4cm square shape.

[0044] The enumerated embodiments are not limited to fabrics of this type of components, and other types of blended fabrics of polyester and cotton in different proportions are also applicable.

[0045] Examples 1-5

[0046] A method for recycling polyester-cotton blended fabrics comprises the following steps:

[0047] S1. 10g of polyester-cotton blended fabric was washed with methanol at 50°C for 60 minutes. During the washing process, 0.2g of cetostearyl phosphate was added for washing. After washing, the fabric was dried at 70°C for 1 hour. The dried blended fabric, 40g of methanol, 1g of dimorpholinyl diethyl ether, and 1g of auxiliary catalyst were added to a reactor. The reactor was then heated to 65°C. After reacting for 3 hours, the reactor was cooled to room temperature. The remaining block solid in the reactor was taken out. The block solid was an undamaged cotton fiber frame, and the liquid was a slurry. The type and amount of the auxiliary catalyst in Examples 1-5 are shown in Table 1.

[0048] S2. The cotton fiber frame was washed twice with methanol and dried to obtain 4.5 g of cotton fiber frame. All cotton fiber components were retained. The washing liquid was combined with the slurry in the kettle, and the solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer dimethyl terephthalate (DMT, see Figure 1 ); the filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, bismorpholinyl diethyl ether and di[2-(N,N-dimethylaminoethyl)] ether.

[0049] Table 1 Composite components of catalysts in Examples 1-5

[0050]

[0051] Example 6

[0052] A method for recycling polyester-cotton blended fabrics comprises the following steps:

[0053] S1. 10g of polyester-cotton blended fabric was washed with methanol at 70°C for 20 minutes. During the washing process, 0.2g of cetostearyl phosphate was added for washing. After washing, the fabric was dried at 70°C for 1 hour. The dried blended fabric was added into a reactor with 40g of methanol, 2g of N-methylmorpholine, 2g of di[2-(N,N-dimethylaminoethyl)]ether, and 2g of dodecyl sulfopropyl betaine. The reactor was then heated to 40°C. After reacting for 6 hours, the reactor was cooled to room temperature. The remaining block solid in the reactor was taken out. The block solid was an undamaged cotton fiber frame, and the liquid was a slurry.

[0054] S2. The cotton fiber frame was washed twice with methanol and 4.5 g of cotton fiber frame was obtained after drying. All cotton fiber components were retained. The washing liquid was combined with the slurry in the kettle. The solid part and the liquid part in the slurry were separated by filtration. The solid part was the depolymerized polyester monomer DMT. The filtrate was distilled and vacuum distilled to recover methanol, ethylene glycol, N-methylmorpholine and di[2-(N,N-dimethylaminoethyl)] ether.

[0055] Figure 1The hydrogen nuclear magnetic resonance spectrum of the polyester monomer dimethyl terephthalate (DMT) recovered after depolymerization provided in Example 6 of the present invention ( 1 1H NMR).

[0056] Figure 2 The separated and recycled polyester and cotton blended fabric provided in Example 6 of the present invention; wherein A is the blended fabric before the separation reaction; and B is the pure cotton fabric after the separation reaction, in which the cotton fibers are not damaged.

[0057] Example 7

[0058] A method for recycling polyester-cotton blended fabrics comprises the following steps:

[0059] S1. 10g of polyester-cotton blended fabric was washed with methanol at 60°C for 20 minutes. During the washing process, 0.2g of cetostearyl phosphate was added for washing. After washing, the fabric was dried at 70°C for 1 hour. The dried blended fabric was added into a reactor with 40g of methanol, 0.1g of 2-morpholinylpyridine, 1g of di[2-(N,N-dimethylaminoethyl)]ether, and 1g of dodecyl hydroxypropyl phosphate betaine. The reactor was then heated to 90°C. After reacting for 4 hours, the reactor was cooled to room temperature. The remaining block solid in the reactor was taken out. The block solid was an undamaged cotton fiber frame, and the liquid was a slurry.

[0060] S2. The cotton fiber frame is washed twice with methanol and dried to obtain 4.5 g of cotton fiber frame. All cotton fiber components are retained. The washing liquid is combined with the slurry in the kettle. The solid part and the liquid part in the slurry are separated by filtration. The solid part is polyester depolymerized dimethyl phthalate. The filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, 2-morpholinylpyridine and di[2-(N,N-dimethylaminoethyl)] ether.

[0061] Example 8

[0062] A method for recycling polyester-cotton blended fabrics comprises the following steps:

[0063] S1. 10g of polyester-cotton blended fabric was washed with methanol at 60°C for 50 minutes. During the washing process, 0.2g of cetostearyl phosphate was added for washing. After washing, the fabric was dried at 70°C for 1 hour. The dried blended fabric was added into a reactor with 40g of methanol, 1g of 2-morpholinylpyridine, 1g of di[2-(N,N-dimethylaminoethyl)]ether, and 1g of dodecyl hydroxypropyl phosphate betaine. The reactor was then heated to 80°C. After reacting for 2 hours, the reactor was cooled to room temperature. The remaining block solid in the reactor was taken out. The block solid was an undamaged cotton fiber frame, and the liquid was a slurry.

[0064] S2. The cotton fiber frame is washed twice with methanol and dried to obtain 4.5 g of cotton fiber frame. All cotton fiber components are retained. The washing liquid is combined with the slurry in the kettle. The solid part and the liquid part in the slurry are separated by filtration. The solid part is polyester depolymerized dimethyl phthalate. The filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, 2-morpholinylpyridine and di[2-(N,N-dimethylaminoethyl)] ether.

[0065] Example 9

[0066] A method for recycling polyester-cotton blended fabrics comprises the following steps:

[0067] S1. 10g of polyester-cotton blended fabric was washed with methanol at 70°C for 40 minutes. During the washing process, 0.2g of cetostearyl phosphate was added for washing. After washing, the fabric was dried at 70°C for 1 hour. The dried blended fabric was added into a reactor with 40g of methanol, 0.5g of morpholinoacetonitrile, 1g of di[2-(N,N-dimethylaminoethyl)]ether, and 1g of dodecyl hydroxypropyl phosphate betaine. The reactor was then heated to 80°C. After reacting for 4 hours, the reactor was cooled to room temperature. The remaining block solid in the reactor was taken out. The block solid was an undamaged cotton fiber frame, and the liquid was a slurry.

[0068] S2. The cotton fiber frame is washed twice with methanol, and 4.5 g of the cotton fiber frame is obtained after drying. All the cotton fiber components are retained. The washing liquid is combined with the slurry in the kettle, and the solid part and the liquid part in the slurry are separated by filtration. The solid part is polyester depolymerized dimethyl phthalate; the filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, morpholinoacetonitrile and di[2-(N,N-dimethylaminoethyl)] ether.

[0069] Example 10

[0070] A method for recycling polyester-cotton blended fabrics comprises the following steps:

[0071] S1.1 kg of polyester-cotton blended fabric was washed with methanol at 60°C for 50 minutes. During the washing process, 20 g of cetostearyl phosphate was added for washing. After washing, the fabric was dried at 60°C for 1 hour. The dried blended fabric was added into a reactor with 4 kg of methanol, 100 g of 2-morpholinylpyridine, 100 g of di[2-(N,N-dimethylaminoethyl)]ether, and 100 g of dodecyl hydroxypropyl phosphate betaine. The reactor was then heated to 80°C. After reacting for 2 hours, the reactor was cooled to room temperature. The block solid remaining in the reactor was taken out. The block solid was an undamaged cotton fiber frame, and the liquid was a slurry.

[0072] S2. The cotton fiber frame is washed twice with methanol and dried to obtain 450 g of cotton fiber frame. All cotton fiber components are retained. The washing liquid is combined with the slurry in the kettle. The solid part and the liquid part in the slurry are separated by filtration. The solid part is the depolymerized polyester monomer DMT. The filtrate is distilled and vacuum distilled to recover methanol, ethylene glycol, 2-morpholinopyridine and di[2-(N,N-dimethylaminoethyl)] ether.

[0073] Comparative Example 1

[0074] A method for recycling polyester-cotton blended fabrics, the other contents of which are the same as those of Example 1, except that the catalyst used is 2g of dimorpholinyl diethyl ether.

[0075] Comparative Example 2

[0076] A method for recycling polyester-cotton blended fabrics, the other contents of which are the same as those of Example 1, except that the catalyst used is 2g of di[2-(N,N-dimethylaminoethyl)]ether.

[0077] Comparative Example 3

[0078] A method for recycling polyester-cotton blended fabrics, the other contents of which are the same as those of Example 1, except that the catalyst used is 2g of dodecyl dimethyl betaine.

[0079] Test and Evaluation

[0080] The depolymerization efficiency of polyester, the recovery rate of DMT monomer and the recovery rate of cotton components in the test examples and comparative examples are shown in Table 2.

[0081] Among them, the depolymerization efficiency (E) can be calculated from the amount of solids remaining after the reaction. The calculation formula is as follows:

[0082] Depolymerization efficiency (E) = (polyester fiber content in textile fabric - amount of undepolymerized polyester) polyester fiber content in textile fabric.

[0083] Table 2 Component recovery results

[0084]

[0085] The cotton components obtained in the examples and comparative examples were opened by an opener to form cotton fibers. The recycled cotton fibers were made into regenerated cotton yarns, and the physical properties were tested according to GB / T20392 and other standards. The physical properties are shown in Table 3.

[0086] Table 3 Physical properties of regenerated cotton yarn

[0087]

[0088]

[0089] The polyester monomer DMT obtained in Example 1 and Comparative Examples 1-3 was polymerized in vacuum at 290° C. for 3 hours using antimony trioxide as a catalyst to generate polyester. The obtained polyester was repeatedly depolymerized and polymerized multiple times. The parameters of each depolymerization and polycondensation are shown in Table 4.

[0090] Table 4 Parameters of repeated polymerization and depolymerization of polyester depolymerization monomers

[0091]

[0092] The above results show that the catalyst system used in the present invention can achieve 100% depolymerization of polyester under low temperature conditions, and at the same time achieve complete separation of polyester and cotton components in polyester-cotton blended fabrics with a high recovery rate. Moreover, the reaction separation process in the present invention is gentle and efficient, and the cotton fiber can obtain 100% pure components and its fibers are almost not damaged, and can be directly spun into silk threads or used as raw materials to produce regenerated cotton fibers. The recovered polyester depolymerization monomers can also be used for the synthesis of new polyesters, thereby realizing the closed-loop recycling of the two fiber components in polyester-cotton blended waste. The comparative example cannot obtain a pure cotton component without polyester components, nor can it produce regenerated cotton fibers.

[0093] The above are only preferred specific implementations of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for recycling polyester-cotton blended fabrics, characterized in that: The following steps are involved: S1. After washing the polyester-cotton blended fabric with a mixture of alcohol and ester, depolymerization reaction is carried out in an alcohol solution using a composite catalyst to obtain cotton fibers and slurry; the composite catalyst comprises a main catalyst and an auxiliary catalyst; the main catalyst is a morpholine compound, and the auxiliary catalyst is a mixture of a zwitterionic compound and di[2-(N,N-dimethylaminoethyl)] ether; S2. washing the cotton fiber with alcohol to obtain a washing liquid, mixing the washing liquid with the slurry, and performing solid-liquid separation to obtain polyester monomers and a filtrate.

2. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: The morpholine compounds include one or more of morpholine, N-ethylmorpholine, N-methylmorpholine, morpholinoacetonitrile, N-(2-cyanoethyl)morpholine, morpholine-2-carboxylate, 2-morpholinopyridine, and bismorpholinodiethyl ether.

3. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: The zwitterionic compound includes one or more of carboxylic acid betaine, sulfo betaine and phosphate betaine.

4. The method for recycling polyester-cotton blended fabric according to claim 3, characterized in that: The carboxylate betaine includes dodecyl dimethyl betaine, the sulfo betaine includes dodecyl sulfopropyl betaine, and the phosphate betaine includes dodecyl hydroxypropyl phosphate betaine.

5. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: The temperature of the depolymerization reaction is 40-90° C., and the time of the depolymerization reaction is 2-6 hours.

6. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: The dosage of the composite catalyst is 0.1-20% of the mass of the polyester-cotton blended fabric; the mass ratio of the main catalyst to the auxiliary catalyst is 1:1-10, and the mass ratio of the di[2-(N,N-dimethylaminoethyl)]ether to the zwitterionic compound is 1:0.1-10.

7. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: In step S1, the alcohol includes methanol, the ester includes fatty alcohol phosphate, and the washing temperature is 50-70°C.

8. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: The cotton content in the polyester-cotton blended fabric is 5-95%.

9. The method for recycling polyester-cotton blended fabric according to claim 1, characterized in that: The method also includes subjecting the filtrate to atmospheric distillation to recover alcohol, and then subjecting the filtrate to vacuum distillation or extraction to recover the diol monomer of the polyester, as well as morpholine compounds and di[2-(N,N-dimethylaminoethyl)]ether.

10. Recycled cotton fiber and polyester monomers obtained by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for recovery of polyurethane through alcoholysis

    CN102796279A

  • Method for preparing polyol by liquefying waste polyurethane foam

    CN113637221A

  • Recycling method of polyester blended fabric

    CN116655465A

  • Method for degrading and recycling PET (Polyethylene Terephthalate)

    CN117430506A

  • Decomposition method for urethane resin

    JP2006257356A