Forming method for one-cavity multi-die forging hot working
By designing multiple molding process cavity in the same mold and completing forging in one heating, the problems of cumbersome processes and unstable quality in traditional forging methods are solved, and the internal tissue of forging and the improvement of production efficiency are achieved. High-quality production of free forgings in complex shapes.
Patent Information
- Application Number
- CN202411166759.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional forging method for free forging parts with complex shapes has problems such as cumbersome forging processes, multiple heating affects quality, poor consistency, low production efficiency and difficult to guarantee physical and chemical performance, resulting in difficulty in ensuring the internal tissue quality of the forging parts and low product qualification rate.
By adopting one-chamber multi-mode forging hot processing method, by designing multiple corresponding molding step cavity in the same mold and completing all molding steps in one heating, the number of steps and cavity size are reasonably designed, and the number of steps and cavity size are controlled. The final deformation amount is carried out, followed by heat treatment and physical and chemical testing.
Significantly reduce the number of furnace reopening and emptying phenomena, improve the internal tissue structure of forgings, simplify production processes, improve production efficiency and product qualification rate, and ensure that the quality and performance of forgings meet the needs of high-demand industries.
Smart Images

Figure CN118893167A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of forging hot processing, and in particular relates to a one-cavity multi-die forging hot processing forming method for manufacturing irregular free forgings such as long rods with special-shaped cross-sections. Background Art
[0002] In the field of aero-engine manufacturing, 1C11N2WMoVNb material, as a martensitic stainless steel, is widely used in the manufacture of key components such as blades, blisks, and journals. Such components usually require complex-shaped free forgings, which have extremely high requirements for internal organization and performance and require 100% performance and organization inspection. The traditional forging method of complex-shaped free forgings has the following problems:
[0003] The forging process is complicated: multiple forging steps are designed according to the different cross-sections of the forgings, and each step requires a separate mold, which increases production complexity and cost;
[0004] Multiple heating affects quality: After each process step is completed, the unforged part needs to be returned to the furnace for heating, resulting in multiple empty firings, which has an adverse effect on the overall internal structure and performance of the forging;
[0005] Poor consistency: Manual operation during the billet making process leads to poor product consistency, affecting the quality of the final product;
[0006] Low production efficiency: Multiple steps, multiple heating and cooling processes will extend the production cycle and reduce production efficiency;
[0007] Physical and chemical properties are difficult to guarantee: Due to repeated heating and empty firing, the physical and chemical properties of forgings are difficult to meet the design requirements, increasing the risk of scrapping.
[0008] The above problems make it difficult to ensure the internal structure quality of forgings, and the physical and chemical test results are often unqualified, which will seriously affect the product's qualification rate and performance stability.
[0009] Therefore, a new forging method is urgently needed to solve the forming problem of free forgings with complex shapes, so as to improve the internal structure of forgings, improve the physical and chemical properties, simplify the production process and improve production efficiency. Summary of the invention
[0010] The purpose of the present invention is to provide a one-cavity multi-die forging hot working forming method to solve the problems of poor internal structure of forgings, unqualified physical and chemical tests, etc. caused by multiple forging steps, multiple fires, and empty furnace burning in the prior art.
[0011] In order to achieve the above object, the present invention provides a one-cavity multi-die forging hot working forming method, comprising the following steps:
[0012] Step 1: design multiple forming steps according to the forging structure; Step 2: design multiple cavities corresponding to the forming steps in the same mold; Step 3: make a mold containing multiple cavities; Step 4: heat the raw materials and put them into the mold; Step 5: complete the forging of all forming steps in one heating.
[0013] Furthermore, the forging structure includes a first end, a rod forging and a second end; the first end and the second end are connected through the rod forging.
[0014] Further, a size of the first end is smaller than a size of the second end, and the first end and the second end have the same shape.
[0015] Furthermore, in step 1, the design of the forming process follows the following principles: the number of process steps M≤4; the connecting portion adjacent to the first end and the rod forging can be combined into the same forging process; the connecting portion adjacent to the rod forging and the second end can also be combined into the same forging process.
[0016] Specifically, in step 2, the cavity design follows the following principles: the length of the rod forging is based on the nominal size Ln, the process step of the nominal size Ln = L nominal + 1 / 2 nominal size positive difference; the process step of the rod forging diameter Φn = Φn nominal + 2 / 3 nominal size positive difference; the thickness size δn of the rod forging = δ nominal + positive difference.
[0017] Furthermore, in step three, the production of the mold includes: determining the maximum working projection area and height dimensions of the mold; and producing a plurality of process step cavities on the working plane of the mold.
[0018] Specifically, in the step three, the design of the process cavity includes: after the upper and lower anvils are molded together, the cavity completely conforms to the size of the blanking rod forging and the size of the first end and the second end; the size of the first end and the second end is generally L1 head blanking = (1 / 3-1 / 4) * L1 head cavity; the cavity size is enlarged to 1.01%-1.02% of the material shrinkage rate μ; and a rounded transition is applied at the cavity opening.
[0019] Furthermore, in step five, the final deformation amount is 25%-30%.
[0020] In addition, the present invention also includes the step of post-processing the forging, and the post-processing includes: sandblasting and grinding the forging structure; and checking whether the size of the forging structure meets the requirements.
[0021] Furthermore, the present invention also includes heat treatment steps: annealing, keeping warm at 800-1000°C for 110-130 minutes and then air cooling; solution treatment, keeping warm at 1020-1060°C for 50-65 minutes and then air cooling; and physical and chemical testing steps.
[0022] Specifically, the method is used to produce irregular free forgings such as long rods with special-shaped cross-sections.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] By designing multiple cavities corresponding to the forming steps in the same mold and completing the forging of all the forming steps in one heating, the present invention can significantly reduce the number of re-melting and empty burning phenomena, and can effectively improve the internal organizational structure of the forging structure. This method can not only simplify the production process, but also shorten the production cycle, and can also improve the qualified rate of the forging structure, and is particularly suitable for the production of free forgings with complex shapes.
[0025] Furthermore, the present invention can further optimize the forging process by reasonably designing the number of process steps, cavity size and shape, and controlling the final deformation. At the same time, the quality and performance of the forging structure can be ensured through subsequent heat treatment and physical and chemical testing steps. This comprehensive process design and quality control method makes the present invention particularly suitable for making irregular free forgings such as long rods with special cross-sections, meeting the needs of high-demand industries such as aviation and energy. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a schematic diagram of a forging in one embodiment of the present invention;
[0027] Figure 2 A schematic diagram of a special anvil in one embodiment of the present invention;
[0028] Figure 3 This is a schematic diagram from another perspective of making a special anvil in one embodiment of the present invention.
[0029] In the figure, 1, Q1 area; 2, Q2 area; 3, Q3 area; 4, making a special anvil. DETAILED DESCRIPTION
[0030] The following is a more detailed description of a one-cavity multi-die forging hot working forming method of the present invention, wherein the preferred embodiment of the present invention is shown, and it should be understood that those skilled in the art can modify the present invention described herein and still achieve the advantageous effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art and not as a limitation of the present invention.
[0031] In the description of this specification, "one embodiment" or "some embodiments" etc. means that one or more embodiments of this specification include a specific feature, structure or characteristic described in conjunction with the embodiment. Therefore, the phrases "in one embodiment", "in some embodiments", "in some other embodiments", "in some other embodiments", etc. appearing in different places in this specification do not necessarily refer to the same embodiment, but mean "one or more but not all embodiments", unless otherwise specifically emphasized in other ways.
[0032] The present invention is described in more detail by way of example in the following paragraphs. Advantages and features of the present invention will become more apparent from the following description.
[0033] The present invention proposes a one-cavity multi-die forging hot processing forming method, which is particularly suitable for the processing of martensitic stainless steels such as 1C11N2WMoVNb materials. 1C11N2WMoVNb material is a high-performance martensitic stainless steel, mainly used for key components such as aircraft engine blades, blisks, shaft necks, engine suspensions, etc. This material exhibits excellent comprehensive mechanical properties when working in a humid environment below 600°C, and has high thermal strength, good stress corrosion resistance and hot and cold processing properties. The method of the present invention aims to solve the problems of uneven structure and unstable performance caused by multiple remelting and empty firing in traditional forging processes, and provide better quality forgings for high-demand industries such as aerospace.
[0034] Specifically, in this embodiment, the one-cavity multi-die forging hot working forming method comprises the following steps:
[0035] Step 1: Design multiple forming steps according to the forging structure;
[0036] Step 2: designing multiple cavities corresponding to the molding steps in the same mold;
[0037] Step 3: making a mold including a plurality of the cavities;
[0038] Step 4, heating the raw materials and placing them into the mold;
[0039] Step 5: Complete the forging of all forming steps in one heating.
[0040] In step one, first, the forging section is divided according to the required forging structure. The principle of division is to maximize the mold requirements for the cross-section of the forging structure while meeting the maximum forging resistance. Preferably, the forging structure can be divided into three areas: the first end, which is defined as Q1 area 1 (i.e., the large head part of the forging structure) in this embodiment, the rod forging Q2 area 2 (the rod part of the forging connecting rod) and the second end, which is defined as Q3 area 3 (the small head part of the forging connecting rod) in this embodiment. Figure 1 As shown, the forging structure consists of these three regions.
[0041] The above classification method for forging structure has the following advantages:
[0042] Accurately control the deformation degree of each part to ensure uniform forming of each part of the forging structure;
[0043] It is conducive to designing a more reasonable forging process and reducing material waste;
[0044] It is convenient to control the temperature of each part to avoid local overheating or too fast cooling;
[0045] Improve the internal quality of forging structure and reduce the occurrence of defects.
[0046] Next, the molding process is designed according to the three areas (Q1 area\Q2 area 2\Q3 area 3) divided above. Preferably, three molding process steps are designed, namely, process step G1, process step G2 and process step G3, corresponding to the Q1 area, the Q2 area and the Q3 area respectively. The design of the molding process follows the following principles:
[0047] a) The number of process steps M≤4;
[0048] b) The connection between the first end and the rod forging can be forged in the same process step; the connection between the rod forging and the second end can also be forged in the same process step (using process residual blocks for natural transition).
[0049] The advantages of the above molding step design are:
[0050] a) Reduce the number of mold changes and improve production efficiency;
[0051] b) Reduce production costs and mold making costs;
[0052] c) Reduce the number of intermediate heating times and reduce energy consumption;
[0053] d) Simplify the production process and improve the consistency of operations.
[0054] In this embodiment, the molds M1, M2, and M3 are designed according to the steps G1, G2, and G3. Figure 2 and Figure 3 As shown, the special anvils 4 required to be manufactured are M1, M2, and M3 from right to left. The cavity design follows the following principles:
[0055] a) The length of the rod forging is based on the nominal size Ln step = L nominal + 1 / 2 nominal size positive difference;
[0056] b) Diameter Φn step = Φn nominal + 2 / 3 nominal size positive difference;
[0057] c) Thickness dimension δn = δ nominal + positive difference.
[0058] Preferably, the nominal size positive difference is +3mm, the diameter positive difference is +4mm, and the thickness positive difference is +5mm.
[0059] The advantages of this design approach are:
[0060] a) The shrinkage and deformation of the material during the forging process are taken into account, and the dimensional accuracy of the forging structure is improved;
[0062] b) Reserve appropriate machining allowance to facilitate subsequent machining;
[0063] c) It is beneficial to control the internal structure of the forging structure and reduce defects;
[0064] d) The versatility of the mold is improved and can be used for the production of forging structures of different sizes and specifications.
[0065] Next, select the appropriate production equipment. Preferably, a 1600T press can be selected. Determine the maximum bearing surface size and maximum projection area of the required mold. Preferably, a length of 1500mm and a width of 1200mm can be selected.
[0066] Then, the maximum working projection area and height of the mold are determined according to the selected production equipment. Preferably, the maximum outline size can be 1500mm in length, 1200mm in width, and 800mm in height.
[0067] Make multiple process cavities on the mold working plane. The design of process cavity includes:
[0068] a) after the upper anvil and the lower anvil are molded together, the die cavity completely conforms to the size of the blanking rod forging and part of the size of the first end and the second end;
[0069] b) The dimensions of the first end and the second end are generally L1 head blank = (1 / 3-1 / 4) * L1 head cavity;
[0070] c) The cavity size is enlarged to 1.01%-1.02% of the material shrinkage μ;
[0071] d) A rounded transition should be applied at the cavity opening.
[0072] Preferably, a suitable fillet transition is applied at the cavity opening: the central axis of the semicircle is aligned with the center line of the cavity length direction, and a tangent line of the semicircle is made at an angle of 40° to 45° on both sides of the center line of the cavity length direction. The intersection of the tangent line and the cavity is represented by R to indicate the diameter of the required material, and a smooth transition is achieved. This design is conducive to material flow and demolding.
[0073] The advantages of the above mold design are:
[0074] a) One set of molds completes multiple steps, reducing mold replacement time and cost;
[0075] b) Taking the shrinkage rate of the material into consideration, the dimensional accuracy of the forging is improved;
[0076] c) The rounded corner transition design is conducive to material flow and reduces forging defects;
[0077] d) Increase the service life of the mold and reduce production costs;
[0078] e) Improves the surface quality of forgings and reduces the workload of subsequent processing.
[0079] The raw material volume required for each molding step is cut according to the conventional method. Preferably, the volume of the material required for each molding step can be:
[0080] G1 = Φ250mm×125mm;
[0081] G2=70mm×((250+150) / 2)mm×(750-25-75)mm;
[0082] G3 = Φ150mm×125mm.
[0083] The heating process is a key step in the forging process. For 1C11N2WMoVNb materials, resistance furnaces or induction heating equipment are usually used for heating. Preferably, the heating temperature is controlled in the range of 1150-1200°C, and the holding time is 1-2 hours. The heating rate needs to be controlled during the heating process to avoid excessive thermal stress that causes material cracking.
[0084] The advantages of heating are:
[0085] a) Improve the plasticity of materials and reduce deformation resistance;
[0086] b) Make the material structure more uniform and improve the forging performance;
[0087] c) It is beneficial to eliminate segregation in materials and improve the quality of forgings;
[0088] d) Promote the recrystallization process and refine the grain structure.
[0089] Under the premise of ensuring the final forging temperature, all the forging steps are completed. Preferably, the final deformation is 25%-30%. During the forging process, the forging temperature range is controlled between 950-1150°C, the single-pass deformation is controlled between 15-20%, and the forging speed is controlled between 0.5-1m / s.
[0090] For 1C11N2WMoVNb material, the following points should be noted during forging:
[0091] a) Control the forging temperature range to avoid excessively high temperature resulting in coarse grains;
[0092] b) Reasonably control the deformation amount of a single pass to avoid internal cracks caused by excessive deformation;
[0093] c) Properly control the forging speed. Too fast will cause stress concentration, and too slow will cause the temperature to drop too quickly.
[0095] d) During the forging process, the position of the forging needs to be adjusted in time to ensure uniform deformation.
[0096] The forging method of completing all forming steps at one time has the following advantages:
[0097] a) Reduce the number of re-melting and reduce energy consumption;
[0098] b) Avoids the problem of grain coarsening caused by multiple heating;
[0099] c) Improved production efficiency and shortened production cycle;
[0100] d) Improved the internal structure of forgings and improved the uniformity of performance;
[0101] e) Reduces oxidation and decarbonization and improves material utilization.
[0102] In addition, the method proposed in this embodiment also includes the following steps:
[0103] The forging structure is post-processed, the post-processing comprising the steps of:
[0104] a) Sand blasting and grinding of forging structure;
[0105] b) Check whether the dimensions of the forging structure meet the requirements.
[0106] The advantages of a post-processing step are:
[0107] a) Sand blasting can remove the oxide scale on the surface of forgings and improve the surface quality;
[0108] b) Grinding can eliminate minor surface defects and improve the appearance of forgings;
[0109] c) Dimensional inspection ensures that the forgings meet the design requirements and provides guarantee for subsequent processing.
[0110] The forging structure is then heat treated. For 1C11N2WMoVNb material, the typical heat treatment process includes:
[0111] Annealing: 800-1000℃ for 110-130 minutes, air cooling. The purpose of normalizing is to refine the grains and eliminate forging stress.
[0112] Solution treatment: 1020-1050℃ for 50-65 minutes, oil cooling. The purpose of quenching is to obtain martensite structure.
[0113] Tempering: 600-650℃ for 120-240 minutes, air cooling. The purpose of tempering is to eliminate internal stress and improve toughness.
[0114] It can be seen that the advantages of heat treatment are:
[0115] a) Adjust the organizational structure of the material to improve strength and toughness;
[0116] b) Eliminate residual stress generated during forging;
[0117] c) Improve the corrosion resistance and wear resistance of materials;
[0118] d) Optimize the comprehensive performance of materials to meet different usage requirements.
[0119] Then the forging structure is subjected to physical and chemical testing, where the specific items and methods of physical and chemical testing depend on the purpose and requirements of the forging, and are conventional means for those skilled in the art, so they will not be described in detail. Common testing items include metallographic inspection, hardness test, tensile test, impact test, fatigue test and non-destructive testing.
[0120] For aircraft engine parts, physical and chemical testing usually includes the following:
[0121] Metallographic examination: observe the microstructure of the material and evaluate the effect of heat treatment.
[0122] Hardness test: Check whether the hardness of the material meets the requirements, usually using a Rockwell hardness tester or a Vickers hardness tester.
[0123] Tensile test: Tests the tensile strength, yield strength and elongation of a material.
[0124] Impact test: To evaluate the toughness of a material, the Charpy impact test is usually used.
[0125] Fatigue testing: checks the performance of materials under cyclic loading, simulating actual use conditions.
[0126] Non-destructive testing: such as ultrasonic testing, to check whether there are defects inside the forging, such as cracks, inclusions, etc.
[0127] Importance of physical and chemical testing:
[0128] a) Ensure that the performance of forgings meets the design requirements;
[0129] b) Discover potential quality problems and avoid failure of parts during use;
[0130] c) Provide reliable data support for product quality;
[0131] d) It helps to optimize the production process and improve the stability of product quality.
[0132] The beneficial effects of the one-cavity multi-die forging hot working forming method proposed in this embodiment are as follows:
[0133] By designing multiple cavities corresponding to the forming steps in the same mold and completing the forging of all the forming steps in one heating, the number of re-melting and the phenomenon of empty burning can be reduced. The internal organizational structure of the forging can be effectively improved, and the uniformity of the forging structure and the stability of performance can be improved.
[0134] This method simplifies the production process, reduces the number of mold changes and intermediate heating times, shortens the production cycle, and improves production efficiency and material utilization. By reasonably designing the number of process steps, cavity size and shape, and controlling the final deformation, this method can optimize the forging process and improve the forming accuracy and surface quality of the forging.
[0135] The method proposed in this embodiment is particularly suitable for making irregular free forgings with special-shaped cross-sections, such as key parts such as aerospace engine blades, blisks, and journals. Subsequent heat treatment and physical and chemical testing steps can ensure that the quality and performance of the forgings meet the needs of high-demand industries. This comprehensive process design and quality control method effectively improves the comprehensive performance of high-performance materials such as 1C11N2WMoVNb.
[0136] By reducing the number of heating times and energy consumption, this method also has the effect of energy saving and emission reduction, which meets the requirements of sustainable development. For 1C11N2WMoVNb material, this method gives full play to its excellent hot processing performance and can obtain a more uniform organizational structure and more stable performance.
[0137] In summary, the present invention provides a higher quality, higher efficiency and lower cost forging production solution for high-demand industries such as aerospace, and has significant technical and economic value. By optimizing the forging process, the reliability and service life of key components are improved, providing important support for the development of high-performance equipment such as aircraft engines.
[0138] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A one-cavity multi-die forging hot working forming method, characterized in that: The following steps are involved: Step 1: Design multiple forming steps according to the forging structure; Step 2: designing multiple cavities corresponding to the molding steps in the same mold; Step 3, making a mold including a plurality of the cavities; Step 4, heating the raw materials and placing them into the mold; Step 5: Complete the forging of all forming steps in one heating.
2. The method according to claim 1, characterized in that The forging structure is an irregular free forging of a long rod with a special-shaped cross-section; the forging structure comprises a first end, a rod forging and a second end; the first end and the second end are connected through the rod forging.
3. The method according to claim 2, characterized in that The first end has a smaller size than the second end, and the first end has the same shape as the second end.
4. The method according to claim 2, characterized in that: In step 1, the design of the molding step follows the following principles: The number of working steps M≤4; The connection portion between the first end and the rod forging is forged in the same process step; the connection portion between the rod forging and the second end is also forged in the same process step.
5. The method according to claim 2, characterized in that: In step 2, the molding cavity design follows the following principles: The length of the rod forging is the nominal size Ln, and Ln=Lnominal+1 / 2 nominal size positive difference; The rod forging is a process step of diameter Φn, wherein Φn=Φn nominal+2 / 3 nominal size positive difference; The thickness dimension of the rod forging is δn, wherein δn=δnominal+positive difference.
6. The method according to claim 2, characterized in that In the step 3, the design of the process cavity includes: After the upper and lower anvils are closed, the cavity meets the size of the blanking rod forging and the size of part of the first end and the second end; The dimensions of the first end and the second end are L1 head blanking, wherein L1 = (1 / 3-1 / 4) * L1 head cavity; The cavity size is enlarged to take the material shrinkage rate μ in the range of 1.01%-1.02%; The cavity opening adopts rounded transition.
7. The method according to claim 1, characterized in that In the step 3, the making of the mold includes: Determine the maximum working projection area and height dimensions of the mold; Create multiple work-step cavities on the mold work plane.
8. The method according to claim 1, characterized in that In the step five, the final deformation amount is 25%-30%.
9. The method according to claim 1, characterized in that: The method also includes a step of post-processing the forged structure, wherein the post-processing includes: sandblasting and grinding the forged structure; and checking whether the size of the forged structure meets the requirements. After the post-processing is completed, the method also includes a heat treatment step: annealing, keeping the temperature at 800-1000°C for 110-130 minutes and then air cooling; solution treatment, keeping the temperature at 1020-1060°C for 50-65 minutes and then air cooling.
10. The method according to claim 9, characterized in that After the heat treatment is completed, a physical and chemical testing step is also included to test the physical and chemical properties of the forging structure.
Citation Information
Patent Citations
Single-anvil zero-blanking once-forming coal-machine scraper forging technique
CN101417312A
Process for forging 4E front shaft by using 10-ton die forging hammer
CN101733357A
Precision forging process for engine connecting rod and precision forging die
CN102049457A
Forging drawing-out method for high-temperature alloy forge piece
CN109175179A
Forming method for improving grain size of martensitic stainless steel journal forging
CN117798296A