High-strength hydrolysis-resistant method for metal powder injection molding and stainless steel part
Through metal powder injection molding technology, combined with the design of hardware, plastic and silicone layers, the problems of insufficient strength and poor hydrolysis resistance of stainless steel parts are solved, and stainless steel parts with high strength and good hydrolysis resistance are achieved, suitable for electronic products.
Patent Information
- Application Number
- CN202410941699.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
The existing metal powder injection molded stainless steel parts have insufficient strength and poor hydrolysis resistance, resulting in waterproofing and reliability problems in electronic products.
Using high-strength hydrolysis-resistant method of metal powder injection molding, the combination of hardware products, plastic and silicone products are formed through injection molding, in-mold molding and LIM molding. The hardware products are used as the skeleton support, the plastic layer is used as the transition layer, and the silicone layer provides water resistance. and waterproof, combined to improve the overall performance of the product.
It achieves high strength and good hydrolysis resistance in electronic products. Waterproof testing and salt spray test prove that the product can maintain waterproof performance in high humidity and salt spray environments to ensure product reliability.
Smart Images

Figure CN118893210A_ABST
Abstract
Description
Technical Field
[0001] The invention patent relates to the technical field of high-strength and hydrolysis-resistant metal powder injection molding, and specifically, to a high-strength and hydrolysis-resistant method for metal powder injection molding and stainless steel parts. Background Art
[0002] Metal powder injection molded stainless steel parts are widely used in the field of electronic products. Most electronic products require certain waterproof performance. To meet the waterproof performance requirements, metal parts on the market are currently often coated with silicone. Although the metal-to-silicone solution can meet the strength requirements, the self-adhesive adhesive used in the metal-to-silicone bonding has poor hydrolysis resistance, and the glue used for bonding has poor hydrolysis resistance. The product is easily hydrolyzed during salt spray testing, resulting in strength failure.
[0003] Alternatively, stainless steel parts are made by combining plastic with silicone. The hydrolysis resistance of stainless steel parts made in this way is better, but the strength is too poor, which will cause problems with the reliability of electronic products. Summary of the invention
[0004] The purpose of the present invention is to provide a high-strength hydrolysis-resistant method and a stainless steel part for metal powder injection molding, aiming to solve the problems of insufficient strength and poor hydrolysis resistance of stainless steel parts molded by metal powder injection molding in the prior art.
[0005] The present invention is achieved by a high-strength hydrolysis-resistant method for metal powder injection molding, the steps are as follows:
[0006] (1) Injection molding: 316L feed material is formed into a green body by injection molding, and the green body is degreased by catalytic degreasing. After the green body is degreased, it is sintered out of the furnace through the process of thermal degreasing and partial pressure sintering in a vacuum sintering furnace to form a hardware product;
[0007] (2) In-mold forming: PC plastic particles are dried and then plasticized by a screw, and the plasticized PC plastic particles are injected into a mold, in which the hardware product is placed, and after cooling and shaping, a product of hardware combined with plastic is formed;
[0008] (3) LIM molding: The proportion of silicone materials is controlled by a quantitative device, and then different silicone materials are mixed by a mixer to form liquid silicone. The liquid silicone is injected into the barrel of an injection molding machine, and the screw injects the liquid silicone into the mold. After the curing reaction, the mold is opened to obtain a product combining hardware, plastic and silicone.
[0009] Furthermore, in step (1), the catalytic degreasing uses nitric acid as a catalyst to decompose POM into formaldehyde, which is volatilized from the green body and burned in the furnace.
[0010] Furthermore, in step (2), the injection pressure of the plasticized material into the mold is in the range of 100 bar to 110 bar.
[0011] Furthermore, in step (2), when the plasticized material is injected into the mold, the temperature of the mold is in the range of 90-100°C.
[0012] Furthermore, the mold includes at least two cavities. In step (2), after the two cavities are molded together, they are cooled for 2-5 seconds to be shaped to obtain a hardware product combined with plastic.
[0013] Furthermore, the silicone material includes polymethylvinylsiloxane raw rubber and polymethylhydrogensiloxane, and the quantitative device is a feeder, which controls the polymethylvinylsiloxane raw rubber and polymethylhydrogensiloxane to enter the mixer in a ratio of 1:1 for sufficient mixing and then enter the barrel of the injection molding machine.
[0014] Furthermore, the polymethylvinylsiloxane raw rubber contains a platinum catalyst.
[0015] Furthermore, the injection pressure range of the screw is 4-12 MPa, during the curing reaction, the temperature range of the mold is 90-200° C., and the curing time is set to 10-15 s.
[0016] Furthermore, the product obtained in step (3) is subjected to a waterproof test and a salt spray test. The waterproof test shows that the waterproof grade of the product can reach grade 8. In the salt spray test, in a closed environment at 35°C ± 2°C, with a humidity of >85%, a NaCl solution with a mass ratio of 5% ± 1%, and a pH value of the NaCl solution in the range of 6.5-7.2 is used. The product is continuously sprayed with salt water using the NaCl solution. As a result, the outermost layer of silicone adhesive does not peel off or separate after 120 hours.
[0017] The high-strength hydrolysis-resistant stainless steel part comprises a hardware layer, a plastic layer and a silicone layer, wherein the plastic layer is sleeved on the hardware layer, and the plastic layer and the hardware layer are fixedly arranged, the silicone layer is sleeved on the plastic layer, and the silicone layer and the plastic layer are fixedly arranged, the hardware layer is used to support and ensure the strength of the product, the plastic layer is used for transition, and the plastic layer and the silicone layer are used together to enhance the water resistance and waterproofness of the product.
[0018] Compared with the prior art, the high-strength and hydrolysis-resistant method for metal powder injection molding and the stainless steel parts provided by the present invention form products combining hardware, plastic and silicone through injection molding, in-mold molding and LIM molding. The hardware is used as a skeleton support on the inside to ensure the strength of the product. The middle plastic layer plays a transitional role, and the plastic layer and the outer silicone layer cooperate with each other to have good hydrolysis resistance, thereby ensuring reliable performance in the field of electronic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the steps of the high-strength and hydrolysis-resistant method for metal powder injection molding provided by the present invention;
[0020] Figure 2 It is a cross-sectional schematic diagram of the high-strength hydrolysis-resistant stainless steel part provided by the present invention. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0022] The implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0023] The same or similar numbers in the drawings of this embodiment correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right" and the like indicate directions or positional relationships based on the directions or positional relationships shown in the drawings, it is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, the terms describing the positional relationship in the drawings are only used for illustrative purposes and cannot be understood as limitations on this patent. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0024] As shown in the drawings, a preferred embodiment of the present invention is provided.
[0025] The high strength and hydrolysis resistance method of metal powder injection molding is as follows:
[0026] (1) Injection molding: 316L feed material is formed into a green body through injection molding, and the green body is degreased by catalytic degreasing. After the green body is degreased, it is sintered out of the furnace through the process of thermal degreasing and partial pressure sintering in a vacuum sintering furnace to form a hardware product;
[0027] (2) In-mold forming: PC plastic particles are dried and then plasticized by a screw, and the plasticized PC plastic particles are injected into the mold. The mold has been placed with hardware products. After cooling and shaping, a product combining hardware products and plastic is formed;
[0028] (3) LIM molding: The proportion of silicone materials is controlled by a quantitative device, and then different silicone materials are mixed through a mixer to form liquid silicone. The liquid silicone is injected into the barrel of the injection molding machine, and the screw injects the liquid silicone into the mold. After the curing reaction, the mold is opened to obtain a product that combines hardware, plastic and silicone.
[0029] The high-strength and hydrolysis-resistant method of metal powder injection molding is formed into a product combining hardware, plastic and silicone by injection molding, in-mold molding and LIM molding. The hardware is used as a skeleton support on the inside to ensure the strength of the product. The middle plastic layer 2 plays a transitional role, and the plastic layer 2 and the outer silicone layer 3 cooperate with each other, having good hydrolysis resistance, thereby ensuring reliable performance in the field of electronic products.
[0030] The stainless steel material may be 17-4PH, 316L or other stainless steel.
[0031] In step (1), catalytic degreasing uses nitric acid as a catalyst to decompose POM into formaldehyde, which is volatilized from the green body and burned in the furnace.
[0032] In step (2), the injection pressure of the plasticized material into the mold is in the range of 100 bar to 110 bar.
[0033] In step (2), when the plasticized material is injected into the mold, the temperature of the mold is in the range of 90-100°C.
[0034] The mold includes at least two cavities. In step (2), after the two cavities are molded together, they are cooled for 2-5 seconds to be shaped to obtain a hardware product combined with plastic.
[0035] The silicone material includes polymethylvinylsiloxane raw rubber and polymethylhydrogensiloxane. The quantitative device is a feeder. The feeder controls the polymethylvinylsiloxane raw rubber and polymethylhydrogensiloxane to enter the mixer in a ratio of 1:1 for full mixing and then enter the barrel of the injection molding machine.
[0036] Polymethylvinylsiloxane rubber contains a platinum catalyst.
[0037] The injection pressure range of the screw is 4-12MPa. During the curing reaction, the temperature range of the mold is 90-200°C, and the curing time is set to 10-15s.
[0038] The product obtained in step (3) is subjected to a waterproof test and a salt spray test. The waterproof test shows that the waterproof grade of the product can reach grade 8. In the salt spray test, in a closed environment at 35°C ± 2°C, with a humidity of >85%, a NaCl solution with a mass ratio of 5% ± 1%, and a pH value of the NaCl solution in the range of 6.5-7.2 is used to continuously spray the product with salt water using the NaCl solution. As a result, the outermost layer of silicone adhesive does not peel off or separate after 120 hours.
[0039] The high-strength hydrolysis-resistant stainless steel parts include a hardware layer 1, a plastic layer 2 and a silicone layer 3. The plastic layer 2 is sleeved on the hardware layer 1, and the plastic layer 2 and the hardware layer 1 are fixedly arranged. The silicone layer 3 is sleeved on the plastic layer 2, and the silicone layer 3 and the plastic layer 2 are fixedly arranged. The hardware layer 1 is used to support and ensure the strength of the product, the plastic layer 2 is used for transition, and the plastic layer 2 and the silicone layer 3 are used together to enhance the water resistance and waterproofness of the product.
[0040] The above-mentioned high-strength hydrolysis-resistant stainless steel parts use a hardware layer 1 as a skeleton support on the inside to ensure product strength, the middle plastic layer 2 plays a transitional role, and the plastic layer 2 and the outer silicone layer 3 cooperate to have good hydrolysis resistance, ensuring reliable performance in the field of electronic products.
[0041] The thickness of each of the hardware layer 1, the plastic layer 2 and the silicone layer 3 is greater than 0.5 mm.
[0042] High-strength hydrolysis-resistant method embodiment 1:
[0043] (1) Injection molding: 316L feed is injected into the green body, and the green body is degreased by catalytic degreasing, using nitric acid as a catalyst to decompose POM into formaldehyde, which is volatilized from the green body and burned in the furnace. After degreasing, it is sintered in a vacuum sintering furnace through hot degreasing, partial pressure sintering and other processes. The maximum sintering temperature is 1380℃, and the holding time is 180min to obtain a dense hardware product.
[0044] (2) In-mold molding: The plastic PC particles are dried in a drying barrel at a temperature of 120°C for 4 hours; then the plastic particles are fed into the barrel of a vertical injection molding machine through an automatic feeding device; the plastic is plasticized by a screw, and the temperature of the screw is set to 255-270°C. The PC plastic is plasticized evenly in the screw, and then injected into a mold with a temperature of 90-100°C at an injection pressure of 100 bar. After the mold is closed, it is cooled for 2-5 seconds to obtain a metal-bonded plastic product; the turntable speed is set to 2500rpm.
[0045] (3) LIM molding: A feeder is used to control the polymethylvinylsiloxane raw rubber, platinum catalyst and polymethylhydrogensiloxane in a 1:1 ratio, and then they are fully mixed through a mixer and enter the barrel of the injection molding machine. The screw injects the liquid silicone into the mold cavity at an injection pressure of 4-12MPa. The mold temperature is 90-200°C, and the liquid silicone undergoes a curing reaction, where the curing time is set to 10-15s. After the mold is opened, a product with a three-layer structure of metal, plastic and silicone is obtained.
[0046] High-strength hydrolysis-resistant method embodiment 2:
[0047] (1) Injection molding: 316L feed is injected into the green body, and the green body is degreased by catalytic degreasing, using nitric acid as a catalyst to decompose POM into formaldehyde, which is volatilized from the green body and burned in the furnace. After degreasing, it is sintered in a vacuum sintering furnace through hot degreasing, partial pressure sintering and other processes. The maximum sintering temperature is 1380℃, and the holding time is 180min to obtain a dense hardware product.
[0048] (2) In-mold molding: The plastic PC particles are dried in a drying barrel at a temperature of 120°C for 4 hours; then the plastic particles are fed into the barrel of a vertical injection molding machine through an automatic feeding device; the plastic is plasticized by a screw, and the temperature of the screw is set to 255-270°C. The PC plastic is plasticized evenly in the screw, and then injected into a mold with a temperature of 90-100°C at an injection pressure of 105 bar. After the mold is closed, it is cooled for 2-5 seconds to obtain a metal-bonded plastic product; the turntable speed is set to 2500rpm.
[0049] (3) LIM molding: A feeder is used to control the polymethylvinylsiloxane raw rubber, platinum catalyst and polymethylhydrogensiloxane in a 1:1 ratio, and then they are fully mixed through a mixer and enter the barrel of the injection molding machine. The screw injects the liquid silicone into the mold cavity at an injection pressure of 4-12MPa. The mold temperature is 90-200°C, and the liquid silicone undergoes a curing reaction, where the curing time is set to 10-15s. After the mold is opened, a product with a three-layer structure of metal, plastic and silicone is obtained.
[0050] High-strength hydrolysis-resistant method embodiment 3:
[0051] (1) Injection molding: 316L feed is injected into the green body, and the green body is degreased by catalytic degreasing, using nitric acid as a catalyst to decompose POM into formaldehyde, which is volatilized from the green body and burned in the furnace. After degreasing, it is sintered in a vacuum sintering furnace through hot degreasing, partial pressure sintering and other processes. The maximum sintering temperature is 1380℃, and the holding time is 180min to obtain a dense hardware product.
[0052] (2) In-mold molding: The plastic PC particles are dried in a drying barrel at a temperature of 120°C for 4 hours; then the plastic particles are fed into the barrel of a vertical injection molding machine through an automatic feeding device; the plastic is plasticized by a screw, and the temperature of the screw is set to 255-270°C. The PC plastic is plasticized evenly in the screw, and then injected into a mold with a temperature of 90-100°C at an injection pressure of 110 bar. After the mold is closed, it is cooled for 2-5 seconds to obtain a metal-bonded plastic product; the turntable speed is set to 2500rpm.
[0053] (3) LIM molding: A feeder is used to control the polymethylvinylsiloxane raw rubber, platinum catalyst and polymethylhydrogensiloxane in a 1:1 ratio, and then they are fully mixed through a mixer and enter the barrel of the injection molding machine. The screw injects the liquid silicone into the mold cavity at an injection pressure of 4-12MPa. The mold temperature is 90-200°C, and the liquid silicone undergoes a curing reaction, where the curing time is set to 10-15s. After the mold is opened, a product with a three-layer structure of metal, plastic and silicone is obtained.
[0054] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength and hydrolysis-resistant method for metal powder injection molding, characterized in that: Here are the steps: (1) Injection molding: 316L feed material is formed into a green body by injection molding, and the green body is degreased by catalytic degreasing. After the green body is degreased, it is sintered out of the furnace through the process of thermal degreasing and partial pressure sintering in a vacuum sintering furnace to form a hardware product; (2) In-mold forming: PC plastic particles are dried and then plasticized by a screw, and the plasticized PC plastic particles are injected into a mold, in which the hardware product is placed, and after cooling and shaping, a product of hardware combined with plastic is formed; (3) LIM molding: The proportion of silicone materials is controlled by a quantitative device, and then different silicone materials are mixed by a mixer to form liquid silicone. The liquid silicone is injected into the barrel of an injection molding machine, and the screw injects the liquid silicone into the mold. After the curing reaction, the mold is opened to obtain a product combining hardware, plastic and silicone.
2. The high-strength and hydrolysis-resistant method for metal powder injection molding according to claim 1, characterized in that: In step (1), the catalytic degreasing uses nitric acid as a catalyst to decompose POM into formaldehyde, which is volatilized from the green body and burned in the furnace.
3. The high-strength and hydrolysis-resistant method for metal powder injection molding according to claim 1, characterized in that: In step (2), the injection pressure of the plasticized material into the mold is in the range of 100 bar to 110 bar.
4. The high-strength and hydrolysis-resistant method for metal powder injection molding according to claim 1, characterized in that: In step (2), when the plasticized material is injected into the mold, the temperature of the mold is in the range of 90-100°C.
5. The high-strength and hydrolysis-resistant method for metal powder injection molding according to claim 1, characterized in that: The mold comprises at least two cavities. In step (2), after the two cavities are molded together, they are cooled for 2-5 seconds to be shaped to obtain a hardware product combined with plastic.
6. The high-strength and hydrolysis-resistant method for metal powder injection molding according to any one of claims 1 to 5, characterized in that: The silicone material includes polymethylvinylsiloxane raw rubber and polymethylhydrogensiloxane. The quantitative device is a feeder. The feeder controls the polymethylvinylsiloxane raw rubber and polymethylhydrogensiloxane to enter the mixer in a ratio of 1:1 for full mixing and then enter the barrel of the injection molding machine.
7. The high-strength and hydrolysis-resistant method for metal powder injection molding according to claim 6, characterized in that: The polymethylvinylsiloxane raw rubber contains a platinum catalyst.
8. The high-strength and hydrolysis-resistant method for metal powder injection molding according to claim 6, characterized in that: The injection pressure range of the screw is 4-12 MPa. During the curing reaction, the temperature range of the mold is 90-200° C., and the curing time is set to 10-15 s.
9. The high-strength and hydrolysis-resistant method for metal powder injection molding according to any one of claims 1 to 5, characterized in that: The product obtained in step (3) is subjected to a waterproof test and a salt spray test. The waterproof test shows that the waterproof grade of the product can reach grade 8. In the salt spray test, in a closed environment at 35°C ± 2°C, with a humidity of >85%, a NaCl solution with a mass ratio of 5% ± 1%, and a pH value of the NaCl solution in the range of 6.5-7.2 is used to continuously spray the product with salt water using the NaCl solution. As a result, the outermost layer of silicone adhesive does not peel off or separate after 120 hours.
10. High-strength hydrolysis-resistant stainless steel parts, characterized in that: It includes a hardware product layer, a plastic layer and a silicone layer, the plastic layer is sleeved on the hardware product layer, and the plastic layer and the hardware product layer are fixedly arranged, the silicone layer is sleeved on the plastic layer, and the silicone layer and the plastic layer are fixedly arranged, the hardware product layer is used to support and ensure the strength of the product, the plastic layer is used for transition, and the plastic layer and the silicone layer are used together to enhance the water resistance and waterproofness of the product.