High-strength fracturing propping agent and preparation method thereof
By calcining and sintering the dry slag of oil-containing rock chips and aluminum slag at high temperature, bubble-free barium feldspar was generated, which solved the problem of insufficient strength of existing proppants under medium and high closing pressure, and achieved the preparation of high-strength fracturing proppants , meet the demand for increasing production of deep well oil wells and reduce resource consumption.
Patent Information
- Application Number
- CN202411018999.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
The proppants in existing oil and gas mining are insufficient under medium and high closing pressures, especially in the development of deep well dense oil layers, which is difficult to meet the demand for oil well production increase, and the supply and demand of bauxite resources are imbalanced, which increases operating costs.
The high-temperature calcination pretreatment is carried out by mixing dry slag with aluminum slag to promote carbonate decomposition and avoid bubble formation. Then granulate and sinter it at high temperature to generate bubble-free barium feldspar, thereby increasing the small particle size proppant strength.
The strength of high-strength fracturing proppants is significantly improved, with a particle size of 40-70 mesh, and the crushing rate at 86Mpa is <9%, the acid solution is <7%, and the spherical degree is >0.9, which meets the demand for oil well production and reduces the Resource consumption.
Smart Images

Figure CN118995188A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas exploitation, and in particular to a high-strength fracturing proppant and a preparation method thereof. Background Art
[0002] Oil is an important strategic resource. my country's proven recoverable reserves, resources and production values are significantly lower than the world average. Effective exploitation and production increase of oil fields are becoming more and more important. Hydraulic fracturing technology is the most commonly used oil well production increase measure, of which proppant is an important component of hydraulic fracturing. The performance of proppant directly affects the production increase capacity of oil wells. With the continuous development of deep wells and tight oil layers, the closing pressure at the bottom of the oil well increases, and the strength requirements for proppant are also increasing.
[0003] At present, the proppants used in oil and gas production can be roughly divided into three categories: quartz sand proppants, artificial ceramsite proppants and coated proppants. Quartz sand proppants are widely distributed, low in price, but low in strength, easy to crush to form crack closure, and cannot be used in medium and high closure fracturing layers; artificial ceramsite proppants are often made of bauxite, which has the advantages of high strength and high conductivity, but bauxite ceramsite proppants have a large density, which will increase operating costs (such as higher requirements for the performance and pumping conditions of fracturing fluids), and the supply and demand of bauxite resources are seriously unbalanced, so it is particularly important to reduce the use of bauxite; coated proppants can better adapt to the complex environment at the bottom of the oil layer, have better acid resistance, strength and conductivity, but the coating increases the process cost and difficulty.
[0004] In the prior art, Chinese patent CN117247282A discloses a microwave sintered oil-based rock debris residue ceramsite proppant and its preparation method, and specifically discloses that the proportion of each component of the ceramsite proppant is recorded by dry mass as follows: oil-based rock debris residue: 40-60 parts, low-grade bauxite: 10-20 parts, waste aluminum ash: 30-40 parts, coal gangue: 5-10 parts, hydrometallurgical manganese slag: 10-15 parts. Its main mineral groups are barium feldspar, corundum and zirconium oxide. Bauxite and waste aluminum ash are used in this invention, but only to enhance the strength of large-particle proppant; in addition, the presence of carbonate ash in waste aluminum ash affects the strength of barium feldspar.
[0005] In view of this, it is of great significance to provide a high-strength fracturing proppant and a preparation method thereof. Summary of the invention
[0006] The invention provides a high-strength fracturing proppant and a preparation method thereof. The high-strength fracturing proppant is prepared from oil-containing rock cuttings dry residue and aluminum slag, can generate celsium feldspar without bubbles, and can improve its strength at a small particle size.
[0007] A method for preparing a high-strength fracturing proppant comprises the following steps: 1) Pretreatment: Take the oil-based rock cuttings dry slag and aluminum slag and mix them evenly, and perform high-temperature calcination pretreatment to obtain pretreated dry slag; 2) Crushing: crushing the pretreated dry residue pretreated in step 1) to obtain dry powder; 3) Granulation: Granulate the dry powder crushed in step 2) to obtain pellets; 4) Sintering: Sinter the pellets granulated in step 3) to obtain high-strength fracturing proppant.
[0008] In a specific embodiment of the present invention, in step 1) pretreatment, the mass ratio of the oil-based rock cuttings dry slag to the aluminum slag is 85-95:5-15.
[0009] In a specific embodiment of the present invention, the chemical composition and content of the oil-based rock cuttings dry residue are as follows: SiO2 30-45wt%, Al2O3 5-15wt%, CaO 10-15wt%, BaSO4 20-35wt%, MgO <3wt%, Fe2O3 <5%.
[0010] In a specific embodiment of the present invention, the chemical composition and content of the aluminum slag are as follows: Al2O3 70-85wt%, Na2O 5-15w%, NaCl 5-10w% and the balance <5wt%.
[0011] In a specific embodiment of the present invention, in step 1) pretreatment, the high temperature calcination temperature is 900-1000° C. and the time is 20-40 min.
[0012] In a specific embodiment of the present invention, step 2) pulverizing is performed to pulverize until the residue on a 500-mesh sieve is ≤5%.
[0013] In a specific embodiment of the present invention, in step 3) granulation, the roundness of the green ball is 0.9-1.0, the sphericity is 0.9-1.0, and the particle size is 40-70 mesh.
[0014] In a specific embodiment of the present invention, step 4) sintering is performed in a rotary kiln.
[0015] In a specific embodiment of the present invention, step 4) sintering, the sintering temperature is 1100-1180° C., and the sintering time is 1-2 hours.
[0016] The high-strength fracturing proppant prepared by the above preparation method has a particle size of 40-70 meshes, a crushing rate of less than 9% at 86 MPa, an acid solution density of less than 7%, and a sphericity of more than 0.9.
[0017] The invention is based on the fact that high barium content in oil-based rock cuttings dry residue and high aluminum content in aluminum slag can form barium feldspar and thus enhance the strength of the fracturing proppant. However, multiple experiments and studies have found that the strength of the fracturing proppant prepared by directly sintering the oil-containing rock cuttings dry residue and aluminum slag is still poor. The inventors found that since both the rock cuttings dry residue and the aluminum slag contain carbonates, direct roasting will simultaneously form carbon dioxide bubbles and barium feldspar, and the bubbles exist in the barium feldspar grains, which will affect the strength of the barium feldspar grains. In view of this, the invention mixes the oil-containing rock cuttings dry residue and the aluminum slag, and then calcines them (calcination temperature < sintering temperature) to promote the decomposition of carbonates without forming barium feldspar. After granulation, sintering is performed at the sintering temperature, so that there are no carbon dioxide bubbles in the formed barium feldspar, so the barium feldspar grains are stable and the strength of the obtained high-strength fracturing proppant is better.
[0018] In the present invention, the chemical reaction formula for generating celsium feldspar during sintering is as follows:
[0019] The beneficial effects of the present invention are: 1. In the preparation method of the high-strength fracturing proppant of the present invention, the oil-based rock cuttings dry residue and the aluminum slag are mixed and then calcined at 900-1000° C., and the carbonate is decomposed, which is beneficial to the formation of celsium feldspar grains in the subsequent sintering process.
[0020] 2. In the preparation method of the high-strength fracturing proppant of the present invention, since the carbonate is decomposed by calcination, there are no bubbles in the grains of celsium feldspar during the sintering process, which ensures the strength of the celsium feldspar and can significantly improve the strength of the small-particle high-strength fracturing proppant.
[0021] 3. The high-strength fracturing proppant prepared by the preparation method of the present invention has a particle size of 40-70 meshes, a crushing rate of less than 9% at 86 MPa, an acid solution concentration of less than 7%, and a sphericity of more than 0.9. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Attached Figure 1 XDR mineral phase diagram provided for a specific embodiment of the present invention; Attached Figure 2 This is an electron microscope scanning image of the high-strength fracturing proppant provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0024] A method for preparing a high-strength fracturing proppant comprises the following steps: 1) Pretreatment: Take the oil-based rock cuttings dry slag and aluminum slag and mix them evenly, and perform high-temperature calcination pretreatment to obtain pretreated dry slag; 2) Crushing: crushing the pretreated dry residue pretreated in step 1) to obtain dry powder; 3) Granulation: Granulate the dry powder crushed in step 2) to obtain pellets; 4) Sintering: Sinter the pellets granulated in step 3) to obtain high-strength fracturing proppant.
[0025] In some examples, in step 1) pretreatment, the mass ratio of the oil-based rock cuttings dry slag to the aluminum slag is 85-95:5-15.
[0026] In some examples, the chemical composition and content of the oil-based rock cuttings dry residue are as follows: SiO2 30-45wt%, Al2O3 5-15wt%, CaO 10-15wt%, BaSO4 20-35wt%, MgO <3wt%, Fe2O3 <5%.
[0027] In some examples, the chemical composition and content of the aluminum slag are as follows: Al2O3 70-85wt%, Na2O 5-15w%, NaCl 5-10w% and the balance ≤5wt%.
[0028] In some examples, in step 1) pretreatment, the high temperature calcination temperature is 900-1000° C. and the time is 20-40 min.
[0029] In some examples, step 2) pulverizing includes pulverizing until the residue on a 500-mesh sieve is less than 5%.
[0030] In some examples, in step 3) granulation, the roundness of the green ball is 0.9-1.0, the sphericity is 0.9-1.0, and the particle size is 40-70 mesh.
[0031] In some examples, step 4) sintering is performed in a rotary kiln.
[0032] In some examples, step 4) sintering, the sintering temperature is 1100-1180° C., and the sintering time is 1-2 hours.
[0033] The high-strength fracturing proppant prepared by the above preparation method has a particle size of 40-70 meshes, a crushing rate of less than 9% at 86 MPa, an acid solution density of less than 7%, and a sphericity of more than 0.9.
[0034] The invention is based on the fact that high barium content in oil-based rock cuttings dry residue and high aluminum content in aluminum slag can form barium feldspar and thus enhance the strength of the fracturing proppant. However, multiple experiments and studies have found that the strength of the fracturing proppant prepared by directly sintering the oil-containing rock cuttings dry residue and aluminum slag is still poor. The inventors found that since both the rock cuttings dry residue and the aluminum slag contain carbonates, direct roasting will simultaneously form carbon dioxide bubbles and barium feldspar, and the bubbles exist in the barium feldspar grains, which will affect the strength of the barium feldspar grains. In view of this, the invention mixes the oil-containing rock cuttings dry residue and the aluminum slag, and then calcines them (calcination temperature < sintering temperature) to promote the decomposition of carbonates without forming barium feldspar. After granulation, sintering is performed at the sintering temperature, so that there are no carbon dioxide bubbles in the formed barium feldspar, so the barium feldspar grains are stable and the strength of the obtained high-strength fracturing proppant is better.
[0035] In the present invention, the chemical reaction formula for generating celsium feldspar during sintering is as follows:
[0036] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0037] In the following embodiments and comparative examples, the oil-based rock cuttings dry residue is the dry residue remaining after the oil-based rock cuttings generated in the mining process are subjected to heat treatment to remove oil and water, and the oil content and water content thereof are both less than 3‰. Example 1
[0038] This embodiment provides a method for preparing a high-strength fracturing proppant, comprising the following steps: 1. Mix the oil-based rock chip dry slag and aluminum slag evenly at a mass ratio of 90:10, and calcine them at 1000℃ for 30min to obtain pre-treated dry slag; 2. Grind the pretreated dry slag to a 500-mesh sieve residue of 4.2% to obtain dry powder; 3. Granulate the dry powder to obtain 40-70 mesh balls; 4. Place the green ball in a rotary kiln, sinter at 1100-1180°C for 1h (there are temperature fluctuations during the sintering process, and the temperature fluctuation range during the 1h sintering process is recorded here), remove it, and quench it in a coolant to ≤60°C to obtain a 40-70 mesh high-strength fracturing proppant. Example 2
[0039] The present embodiment is different from the embodiment 1 in that the sintering temperature is 1140-1180°C. Example 3
[0040] The present embodiment is different from the embodiment 1 in that the sintering temperature is 1100-1140° C. and the sintering time is 2 h. Example 4
[0041] Compared with Example 2, the present embodiment is different in that the mass ratio of the oil-based rock cuttings dry slag to the aluminum slag is 85:15. Example 5
[0042] Compared with Example 3, the present embodiment is different in that the mass ratio of the oil-based rock cuttings dry slag to the aluminum slag is 95:5.
[0043] Comparative Example 1 The difference between this comparative example and Example 3 is that the mass ratio of the oil-based rock cuttings dry slag to the aluminum slag is 97:3.
[0044] Comparative Example 2 The difference between this comparative example and Example 2 is that the mass ratio of oil-based rock cuttings dry slag to aluminum slag is 80:20; and the sintering time is 2 hours.
[0045] Comparative Example 3 The difference between this comparative example and Example 1 is that the sintering temperature is 1050-1100° C. and the sintering time is 2 h.
[0046] Comparative Example 4 The difference between this comparative example and Example 1 is that the sintering temperature is 1190-1230° C. and the sintering time is 0.5 h.
[0047] Comparative Example 5 The difference between this comparative example and Example 1 is that no calcination treatment is performed.
[0048] The performance results of the crushing rate, acid solubility, roundness and sphericity of the high-strength fracturing proppants of Examples 1-5 and Comparative Examples 1-4 are shown in Table 1.
[0049] Table 1
[0050] It can be seen from the experimental results in Table 1 that, compared with Comparative Examples 1-5, the crushing rate of the high-strength fracturing proppants of Examples 1-5 at a closing pressure of 86 MPa meets the requirement of a crushing rate of <9% in SY / T 5108-2014 "Test Method for Performance of Proppants for Hydraulic Fracturing and Gravel Packing Operations"; this indicates that a higher strength fracturing proppant can be obtained by a better mass ratio of oil-based rock cuttings dry slag to aluminum slag and a better sintering temperature.
[0051] The XDR mineral phase results of the high-strength fracturing proppant of Examples 1-4 and Comparative Example 1 are as follows: Figure 1 shown.
[0052] Attached Figure 1In the figure, S1 represents Example 1, S3 represents Example 2, C3 represents Example 3, T1 represents Comparative Example 1, and C4 represents Example 4.
[0053] Example 1 The electron microscope scanning results of the high-strength fracturing proppant are as follows Figure 2 shown.
[0054] Attached Figure 2 Among them, the main constituent elements represented by P4 and P7 are O, Si, Al and Ba.
[0055] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a high-strength fracturing proppant, characterized in that: The following steps are involved: 1) Pretreatment: Take the oil-based rock cuttings dry slag and aluminum slag and mix them evenly, and perform high-temperature calcination pretreatment to obtain pretreated dry slag; 2) Crushing: crushing the pretreated dry residue pretreated in step 1) to obtain dry powder; 3) Granulation: Granulate the dry powder crushed in step 2) to obtain pellets; 4) Sintering: Sinter the pellets granulated in step 3) to obtain high-strength fracturing proppant.
2. The preparation method according to claim 1, characterized in that: Step 1) pretreatment, the mass ratio of the oil-based rock cuttings dry slag to the aluminum slag is 85-95:5-15.
3. The preparation method according to claim 1 or 2, characterized in that: The chemical composition and content of the oil-based rock cuttings dry residue are as follows: SiO2 30-45wt%, Al2O3 5-15wt%, CaO 10-15wt%, BaSO4 20-35wt%, MgO <3wt%, Fe2O3 <5%.
4. The preparation method according to claim 1, characterized in that: The chemical composition and content of the aluminum slag are as follows: Al2O3 70-85wt%, Na2O 5-15w%, NaCl 5-10w% and the balance ≤5wt%.
5. The preparation method according to claim 1, characterized in that: Step 1) pretreatment, the high temperature calcination temperature is 900-1000°C, and the time is 20-40 minutes.
6. The preparation method according to claim 1, characterized in that: Step 2) crushing, wherein the crushing is performed until the residue on a 500-mesh sieve is less than 5%.
7. The preparation method according to claim 1, characterized in that: Step 3) granulation, the roundness of the green ball is 0.9-1.0, the sphericity is 0.9-1.0, and the particle size is 40-70 mesh.
8. The preparation method according to claim 1, characterized in that: Step 4) sintering, wherein the sintering is carried out in a rotary kiln.
9. The preparation method according to claim 1, characterized in that: Step 4) sintering, the sintering temperature is 1100-1180° C., and the sintering time is 1-2 hours.
10. The high-strength fracturing proppant prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The particle size of the high-strength fracturing proppant is 40-70 meshes, the crushing rate at 86 MPa is less than 9%, the acid solution density is less than 7%, and the sphericity is greater than 0.9.
Citation Information
Patent Citations
Petroleum fracturing propping agent prepared from oil shale ash and preparation method of petroleum fracturing propping agent
CN105331355A
High-strength ceramsite fracturing propping agent and preparation method thereof
CN116177883A
Microwave sintering oil-based rock debris residue ceramsite proppant and preparation method thereof
CN117247282A
High-strength fracturing propping agent and preparation method thereof
CN117887444A
Method for preparing low-density proppant by taking oil-based mud wastes as raw materials
US20210040379A1
Cited By
Fracturing propping agent based on oil-based drilling rock debris tailings and preparation method of fracturing propping agent
CN122587695A
Fracturing proppant based on oil-based drilling cuttings tailings and preparation method thereof
CN122587695B
High-strength fracking proppant and preparation method therefor
WO2026026097A1