Welding method for rapidly connecting aluminum oxide ceramic and titanium alloy under assistance of electric field

Through the electric field-assisted rapid connection method, the problem of high temperature and long time connection between alumina ceramics and titanium alloys is solved, efficient and low-cost welding is achieved, and the mechanical properties and scope of application of the welded joints are improved.

CN118893293APending Publication Date: 2024-11-05SOLOMON (CHANGZHOU) ALLOY NEW MATERIAL CO LTD +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410962893.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art has problems of high connection temperature, long time, low efficiency and high cost when connecting alumina ceramics and titanium alloys, and the traditional diffusion connection method has limited applicability to brittle ceramics and plastic metals.

Method used

By using the electric field-assisted rapid connection method, alumina ceramics and titanium alloys are realized by plating a metal layer on the surface of alumina ceramics and applying electric field and pressure in a vacuum heating furnace. diffusion connection.

Benefits of technology

It significantly reduces welding temperature and time, improves welding efficiency and mechanical properties, avoids the formation of interfacial brittle compounds, expands the scope of material application, and reduces equipment performance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893293A_ABST
    Figure CN118893293A_ABST
Patent Text Reader

Abstract

The invention relates to the field of dissimilar material connection, in particular to a welding method for quickly connecting aluminum oxide ceramic and titanium alloy under the assistance of an electric field, which comprises the following steps: firstly, finishing pre-welding preparation work on the aluminum oxide ceramic and the titanium alloy to be welded, and plating a metal layer on the surface to be welded of the aluminum oxide ceramic through a specific plating technology; after assembly, a sample to be welded is fixed in a specific hot-pressing clamp of a vacuum heating furnace, a certain pressure is applied, the temperature is increased to 700-900 DEG C at the temperature increasing rate of 5-15 DEG C / min, heat preservation is conducted for 1-2 h, meanwhile, an electric field is applied, the sample is cooled to 400 DEG C at the cooling rate of 5-10 DEG C / min, then furnace cooling is conducted, diffusion bonding of the aluminum oxide ceramic and the titanium alloy is completed, and the aluminum oxide ceramic and the titanium alloy are obtained. According to the method, high-quality connection of the aluminum oxide ceramic and the titanium alloy is successfully achieved in an electric field assisted diffusion connection mode, the connection temperature and the connection time needed by welding are greatly reduced, and the problems that traditional diffusion welding is low in efficiency, high in production cost and the like are effectively solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of dissimilar material connection, and in particular to an electric field assisted welding method for quickly connecting alumina ceramics and titanium alloys. Background Art

[0002] In recent years, as IGBT (insulated gate bipolar transistor) components continue to develop towards high power, high current density, high integration and miniaturization, the semiconductor industry has put forward more stringent performance requirements on the high temperature stability and high reliability of IGBT modules. Especially in IGBT module components, achieving high-quality connection between metal and ceramic heat dissipation substrate is a technical difficulty in this field.

[0003] Since alumina ceramics have high thermal conductivity and low dielectric constant, they are often used in electronic products such as IGBT. Titanium alloys are often used in human medicine and electronic devices due to their good biocompatibility and metallic properties. In the actual IGBT product structure system, alumina ceramics and titanium alloys are often required to be tightly connected. However, the fatal weakness of titanium alloy materials is their poor oxidation and corrosion resistance. Therefore, the connection between alumina ceramics and titanium alloys is mostly completed under vacuum conditions. The main connection technologies are: solid-phase diffusion connection, instantaneous liquid phase connection, indirect brazing connection, and active brazing connection. Among them, diffusion welding has the advantages of high flexibility and good connection quality, and is widely used in the connection of ceramic and metal parts in IGBT modules.

[0004] The ideal connection method for electronic components should have the characteristics of low temperature, low cost, high efficiency and high reliability. However, the traditional diffusion connection method has disadvantages such as high connection temperature, long connection time and large energy loss. Therefore, developing a fast connection and high reliability alumina ceramic and titanium alloy connection technology is a technical problem to be solved urgently in the present invention.

[0005] The invention patent with publication number CN112109393B discloses an alumina / nickel-titanium alloy / alumina composite material prepared by diffusion bonding and a method thereof. The invention uses nickel-titanium alloy sheets and alumina sheets as raw materials, and prepares a composite layered sample with a sandwich structure by diffusion bonding under heat treatment conditions of 1250-1500°C, thereby improving the connection quality of alumina ceramics and nickel-titanium alloys. Although this scheme can achieve the connection between alumina ceramics and metals, its disadvantage is that the connection temperature of this method is high and the connection time is long, which greatly accelerates the thermal damage of the material. Moreover, this type of conventional diffusion bonding technology generally has problems such as low welding efficiency and high pressure on the sample to be welded, making it difficult to be widely used in the field of brittle ceramic and plastic metal connection.

[0006] The invention patent with publication number CN112620913A discloses a surface activated aluminum alloy current-assisted non-vacuum diffusion welding method. In order to improve the mechanical properties and metallurgical bonding effect of aluminum alloy joints, the invention pre-plates a layer of activated nanoscale copper film on the surface of the aluminum alloy to be welded by electrodeposition, and uses current to assist in the connection of aluminum alloys and dissimilar metals under non-vacuum conditions. The invention effectively improves production efficiency through electric field assisted welding and can be applied to the field of aluminum alloy welding. The disadvantage is that the coating material used in this method is single, the application range of welding materials is limited, and the substitutability is strong. In addition, this method is not suitable for the connection of alumina ceramics and titanium alloys, and Ti-Cu binary brittle compounds are easily produced at the formed joint interface, thereby deteriorating the mechanical properties of the joint.

[0007] The invention patent with publication number CN106946584A discloses a method for low-temperature rapid welding between ceramics or ceramic-based composite materials and metals. The invention realizes low-temperature rapid welding between zirconium oxide or zirconium oxide-based composite materials and metals in the temperature range of 500-1200°C by applying a current density higher than the critical value to the sample, effectively improving the connection efficiency between metal and ceramic materials. This method can achieve good connection with zirconium oxide-based ceramics with high ionic conductivity by using a small voltage and a large current. However, when welding ceramics with strong electrical insulation, the voltage and power requirements of the equipment are relatively high, which limits the scope of application of this method.

[0008] Therefore, according to the above-mentioned related technologies, it is urgent to develop an electric field assisted welding method for quickly connecting alumina ceramics and titanium alloys. Summary of the invention

[0009] In view of this, the object of the present invention is to provide an electric field assisted rapid connection welding method of alumina ceramics and titanium alloys, so as to improve the mechanical properties and welding efficiency of the welded joint.

[0010] Based on the above purpose, the present invention provides an electric field assisted welding method for quickly connecting alumina ceramics and titanium alloy.

[0011] An electric field assisted rapid welding method for connecting alumina ceramics and titanium alloys comprises the following steps:

[0012] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0013] Step S2. Ceramic surface coating: a metal layer is coated on the surface of the alumina ceramic to be welded by magnetron sputtering, and ultrasonic cleaning is performed, and the surface is dried for standby use;

[0014] Step S3. Pre-welding assembly and debugging: clamp the base metal by a special welding fixture, and make the power supply electrode wire and the base metal tightly contact, and then fix the fixture and the wire in a vacuum heating furnace;

[0015] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 5-15℃ / min, the temperature is raised to 700-900℃, and then kept warm for 1-2h at a pressure of 1-4MPa, and an electric field is applied at the same time. After completion, the cooling rate is controlled to 5-10℃ / min, and after cooling to 400℃, the furnace is cooled to complete the diffusion connection between the alumina ceramic and the titanium alloy.

[0016] Preferably, the metal layer of the ceramic surface coating in step S2 is any one of a Mo layer and a Nb layer.

[0017] Preferably, the thickness of the metal layer in step S2 is 10-20 μm.

[0018] Preferably, in step S3, the two ends of the power electrode wire are respectively connected to the two ends of the alumina ceramic base material and the titanium alloy to be welded, and the current is conducted from the alumina ceramic side to the titanium alloy side.

[0019] Preferably, the current density of the electric field in step S4 is 10-100 mA / mm 2 , the applied voltage is 400-1000V.

[0020] Preferably, the electric field in step S4 is maintained for 10-20 minutes.

[0021] Preferably, the type of the electric field is any one of direct current, alternating current and pulse current.

[0022] Preferably, the coating method in step S2 is magnetron sputtering.

[0023] For the diffusion welding of alumina ceramics and titanium alloys, since the melting point of alumina ceramics (2054℃) is much higher than that of titanium alloys (1670℃), the physical and chemical properties of alumina ceramics are much more stable than those of titanium alloys. During the diffusion welding process of alumina ceramics and titanium alloys, the local plastic deformation of the titanium alloy is mainly relied on to achieve close contact of the interface. Therefore, when selecting welding parameters, the properties of the titanium alloy are mainly considered.

[0024] According to the selection principle of diffusion welding temperature, the welding temperature range should be 0.6Tm-0.8Tm. The melting point Tm of titanium alloy is about 1670℃. According to the selection principle, that is, 1000℃-1350℃, titanium alloy is an α+β dual-phase material. When the temperature reaches 882℃, the α phase will transform into the β phase; when it exceeds 900℃, the microstructure and mechanical properties of the titanium alloy will drop sharply. Therefore, in order not to affect the microstructure and mechanical properties of the parent material and to ensure the activity of the atoms, the diffusion welding temperature is selected to be 700-900℃. At the same time, in order to ensure the full diffusion and interface reaction of atoms during welding and obtain an interface reaction layer of suitable thickness, a relatively long insulation time of 1-2h is required.

[0025] In addition, due to the good plasticity of titanium alloy and low high temperature strength, the yield strength of titanium alloy is only about 50MPa at 800℃. Therefore, when performing diffusion welding of TC4, the connection pressure should not be too large, otherwise it will cause large deformation of the parent material. When the connection pressure is 1-4MPa, the deformation of titanium alloy is very small, while ensuring close contact with alumina ceramics at the interface. Therefore, the connection pressure is selected to be 1-4MPa.

[0026] Beneficial effects of the present invention:

[0027] The present invention successfully achieves high-quality connection between alumina ceramics and titanium alloys through electric field-assisted diffusion connection, greatly reduces the connection temperature and time required for welding, and effectively solves the problems of low efficiency and high production cost of traditional diffusion welding.

[0028] The present invention can avoid the generation of an interface brittle Ti-Al-O ternary compound layer by pre-plating a metal layer on the surface of the alumina ceramic, thereby improving the mechanical properties of the diffusion welding joint, obtaining a full solid solution joint with high mechanical properties, and significantly improving the service performance of the alumina ceramic and titanium alloy diffusion welding joint. In addition, the use of a pre-plating method can expand the application scope of electric field assisted diffusion bonding materials and effectively reduce the performance requirements for equipment.

[0029] The present invention can regulate the type, thickness and distribution of the interface diffusion layer of the diffusion welding joint by adjusting the coating type, power supply parameters and temperature parameters, thereby improving the mechanical properties of the joint and minimizing the thermal damage behavior of the welding temperature to the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 A schematic diagram of electric field assisted diffusion connection in the present invention;

[0032] Figure 2 This is a microscopic morphology of the alumina ceramic / titanium alloy vacuum diffusion welding joint obtained in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0034] Embodiment 1: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0035] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0036] Step S2. Ceramic surface coating: a Mo layer with a thickness of 10 μm is plated on the surface of the alumina ceramic to be welded by magnetron sputtering, and then ultrasonic cleaning is completed and the ceramic is dried for standby use;

[0037] Step S3. Assembly and debugging before welding: clamp the base material by a special welding fixture, and fasten the two ends of the power supply electrode wire to the welding surface of the alumina ceramic base material and the welding surface of the titanium alloy base material, respectively, and then fix the fixture and the wire in a vacuum heating furnace;

[0038] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 5℃ / min, the temperature is raised to 700℃, and then the temperature is kept at 1MPa for 1h, and direct current is applied at the same time, and the current density is 10mA / mm 2 The applied voltage is 400 V, the electric field is maintained for 10 min, and after completion, the cooling rate is controlled to 5 ° C / min. After cooling to 400 ° C, it is cooled with the furnace to complete the diffusion connection between alumina ceramics and titanium alloy.

[0039] Embodiment 2: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0040] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0041] Step S2. Ceramic surface coating: a Nb layer with a thickness of 12 μm is plated on the surface of the alumina ceramic to be welded by magnetron sputtering, and then ultrasonic cleaning is performed and the ceramic is dried for standby use;

[0042] Step S3. Assembly and debugging before welding: clamp the base material by a special welding fixture, and fasten the two ends of the power supply electrode wire to the welding surface of the alumina ceramic base material and the welding surface of the titanium alloy base material, respectively, and then fix the fixture and the wire in a vacuum heating furnace;

[0043] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 7°C / min, the temperature is raised to 740°C, and then the temperature is kept at 2MPa for 1h, and AC is applied at the same time, and the current density is 28mA / mm 2 The applied voltage is 520V, the electric field is maintained for 12min, and after completion, the cooling rate is controlled to be 6℃ / min. After cooling to 400℃, it is cooled with the furnace to complete the diffusion connection between alumina ceramics and titanium alloy.

[0044] Embodiment 3: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0045] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0046] Step S2. Ceramic surface coating: a Mo layer with a thickness of 14 μm is plated on the surface of the alumina ceramic to be welded by magnetron sputtering, and then ultrasonic cleaning is completed and the ceramic is dried for standby use;

[0047] Step S3. Assembly and debugging before welding: clamp the base material by a special welding fixture, and fasten the two ends of the power supply electrode wire to the welding surface of the alumina ceramic base material and the welding surface of the titanium alloy base material, respectively, and then fix the fixture and the wire in a vacuum heating furnace;

[0048] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 9°C / min, the temperature is raised to 780°C, and then the temperature is kept at 3MPa for 1.5h, and a pulse current is applied at the same time, and the current density is 46mA / mm 2 The applied voltage was 640 V, the electric field was maintained for 14 min, and after completion, the cooling rate was controlled at 7 °C / min. After cooling to 400 °C, the furnace was cooled to complete the diffusion connection between the alumina ceramic and the titanium alloy.

[0049] Embodiment 4: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0050] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0051] Step S2. Ceramic surface coating: a Nb layer with a thickness of 16 μm is plated on the surface of the alumina ceramic to be welded by magnetron sputtering, and then ultrasonic cleaning is performed and the ceramic is dried for standby use;

[0052] Step S3. Assembly and debugging before welding: clamp the base material by a special welding fixture, and fasten the two ends of the power supply electrode wire to the welding surface of the alumina ceramic base material and the welding surface of the titanium alloy base material, respectively, and then fix the fixture and the wire in a vacuum heating furnace;

[0053] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 11℃ / min, the temperature is raised to 820℃, and then the temperature is kept at 4MPa for 2h, and direct current is applied at the same time, and the current density is 64mA / mm 2 The applied voltage was 760 V, the electric field was maintained for 16 min, and after completion, the cooling rate was controlled to 8 °C / min. After cooling to 400 °C, the furnace was cooled to complete the diffusion bonding of alumina ceramics and titanium alloy.

[0054] Embodiment 5: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0055] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0056] Step S2. Ceramic surface coating: a Mo layer with a thickness of 18 μm is plated on the surface of the alumina ceramic to be welded by magnetron sputtering, and ultrasonic cleaning is completed, and the ceramic is dried for standby use;

[0057] Step S3. Assembly and debugging before welding: clamp the base material by a special welding fixture, and fasten the two ends of the power supply electrode wire to the welding surface of the alumina ceramic base material and the welding surface of the titanium alloy base material, respectively, and then fix the fixture and the wire in a vacuum heating furnace;

[0058] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 13℃ / min, the temperature is raised to 860℃, and then the temperature is kept at 1MPa for 2h, while applying AC current with a current density of 82mA / mm 2 The applied voltage was 880 V, the electric field was maintained for 18 min, and the cooling rate was controlled at 9 °C / min. After cooling to 400 °C, the furnace was cooled to complete the diffusion connection between alumina ceramics and titanium alloy.

[0059] Embodiment 6: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0060] Step S1. Cleaning the sample before welding: mechanically grind and polish the two base material surfaces to be welded, complete ultrasonic cleaning, and blow dry for standby use;

[0061] Step S2. Ceramic surface coating: a Nb layer with a thickness of 20 μm is plated on the surface of the alumina ceramic to be welded by magnetron sputtering, and then ultrasonic cleaning is performed and the ceramic is dried for standby use;

[0062] Step S3. Assembly and debugging before welding: clamp the base material by a special welding fixture, and fasten the two ends of the power supply electrode wire to the welding surface of the alumina ceramic base material and the welding surface of the titanium alloy base material, respectively, and then fix the fixture and the wire in a vacuum heating furnace;

[0063] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 15℃ / min, the temperature is raised to 900℃, and then the temperature is kept at 2MPa for 2h, and a pulse current is applied at the same time, and the current density is 100mA / mm 2 The applied voltage is 1000V, the electric field is maintained for 20min, and after completion, the cooling rate is controlled to be 10℃ / min. After cooling to 400℃, the furnace is cooled to complete the diffusion bonding of alumina ceramics and titanium alloy.

[0064] Comparative Example 1: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0065] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic treatment, and drying them for later use;

[0066] Step S2. Assembly and debugging before welding: clamp the uncoated alumina ceramic base material and the titanium alloy base material with a special welding fixture, and firmly contact the power electrode wire with the alumina ceramic base material and the titanium alloy base material to be welded, and then put the fixture and the power electrode wire into a vacuum diffusion heating furnace;

[0067] Step S3. Set the diffusion welding process parameters and power supply parameters: the heating rate is 10℃ / min, the temperature is raised to 850℃, and then a pressure of 3MPa is applied, and the temperature is kept for 2h without applying an electric field. After completion, the cooling rate is controlled to 5℃ / min, and after cooling to 400℃, the furnace is cooled to complete the diffusion connection of alumina ceramics and titanium alloy.

[0068] Comparative Example 2: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0069] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic treatment, and drying them for standby use;

[0070] Step S2. Ceramic surface coating: a metal Mo layer with a thickness of 10 μm is coated on the surface of the alumina ceramic to be welded by magnetron sputtering technology, and then ultrasonic treatment is completed and the layer is dried for standby use;

[0071] Step S3. Pre-welding assembly and debugging: clamp the base material with a special welding fixture, and fasten the power electrode wire to the alumina ceramic base material and the titanium alloy base material, and then fix the fixture and the power electrode wire in a vacuum heating furnace;

[0072] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 10℃ / min, the temperature is raised to 1000℃, and then a pressure of 1MPa is applied, and the temperature is kept for 1h. After reaching the predetermined diffusion temperature, the electric field is applied, and the DC current density is 50mA / mm 2 , apply a voltage of 500V, and power on for 5 minutes. After completing the above steps, control the cooling rate to 5℃ / min, cool to 400℃ and then cool with the furnace to complete the diffusion bonding of alumina ceramics and titanium alloy.

[0073] Comparative Example 3: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0074] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic cleaning, and drying them for standby use;

[0075] Step S2. Spray coating on the ceramic surface: a 10 μm thick metal Nb layer is coated on the surface of the alumina ceramic to be welded by magnetron sputtering technology, and then ultrasonic cleaning is completed and the ceramic is dried for standby use;

[0076] Step S3. Pre-welding assembly and debugging: clamp the base material with a special welding fixture, and fasten the power electrode wire to the alumina ceramic base material and the titanium alloy base material, and then put the fixture and the power electrode wire into a vacuum heating furnace;

[0077] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 10℃ / min, the temperature is raised to 600℃, and then a pressure of 1MPa is applied, and the temperature is kept for 1h. After reaching the predetermined diffusion temperature, the electric field is applied, and the DC current density is 50mA / mm 2 , apply a voltage of 500V, and power on for 5 minutes. After completing the above steps, control the cooling rate to 5℃ / min. After cooling to 400℃, cool with the furnace to complete the diffusion connection between alumina ceramics and titanium alloy.

[0078] Comparative Example 4: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0079] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic cleaning, and drying them for later use;

[0080] Step S2. Spray coating on the ceramic surface: using electrophoretic deposition technology to coat a metal Nb layer with a thickness of about 5 μm on the surface of the alumina ceramic to be welded, and then completing ultrasonic cleaning treatment and drying for standby use;

[0081] Step S3. Pre-welding assembly and debugging: clamp the base material with a special welding fixture, and fasten the power electrode wire to the alumina ceramic base material and the titanium alloy base material, and then put the fixture and the power electrode wire into a vacuum diffusion heating furnace;

[0082] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 15℃ / min, the temperature is raised to 750℃, and then a pressure of 1MPa is applied, and the temperature is kept for 0min. After reaching the predetermined diffusion temperature, the electric field is applied, and the pulse current density is 70mA / mm 2 , the applied voltage is 800V, and the power is on for 20 minutes. After completing the above steps, the cooling rate is controlled to 5℃ / min. After cooling to 400℃, it is cooled with the furnace to finally complete the diffusion bonding of alumina ceramics and titanium alloy.

[0083] Comparative Example 5: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0084] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic cleaning, and drying them for later use;

[0085] Step S2. Spray coating on the ceramic surface: using magnetron sputtering technology to coat a metal Nb layer with a thickness of about 5 μm on the surface of the alumina ceramic to be welded, and then completing ultrasonic cleaning treatment and drying for standby use;

[0086] Step S3. Pre-welding assembly and debugging: clamp the base material with a special welding fixture, and fasten the power electrode wire to the alumina ceramic base material and the titanium alloy base material, and then put the fixture and the power electrode wire into a vacuum diffusion heating furnace;

[0087] Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 15℃ / min, the temperature is raised to 700℃, and then a pressure of 1MPa is applied, and the temperature is kept for 3h. After reaching the predetermined diffusion temperature, the electric field is applied, and the DC current density is 100mA / mm 2 , apply a voltage of 1000V, and power on for 20 minutes. After completing the above steps, control the cooling rate to 5℃ / min. After cooling to 400℃, cool with the furnace to complete the diffusion connection between alumina ceramics and titanium alloy.

[0088] Comparative Example 6: A method for welding alumina ceramic and titanium alloy by electric field assisted rapid connection, comprising the following steps:

[0089] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic treatment, and drying them for later use;

[0090] Step S2. Assembly and debugging before welding: clamp the uncoated alumina ceramic base material and the titanium alloy base material with a special welding fixture, and firmly contact the power electrode wire with the alumina ceramic base material and the titanium alloy base material to be welded, and then put the fixture and the power electrode wire into a vacuum diffusion heating furnace;

[0091] Step S3. Set the diffusion welding process parameters and power supply parameters: the heating rate is 10℃ / min, the temperature is raised to 850℃, and then a pressure of 0.3MPa is applied, and the temperature is kept for 2h without applying an electric field. After completion, the cooling rate is controlled to 5℃ / min, and after cooling to 400℃, the furnace is cooled to complete the diffusion connection of alumina ceramics and titanium alloy.

[0092] Comparative Example 7: An electric field assisted rapid connection welding method of alumina ceramic and titanium alloy, comprising the following steps:

[0093] Step S1. Cleaning the sample before welding: mechanically grinding and polishing the surfaces of the two base materials to be welded, and completing ultrasonic treatment, and drying them for later use;

[0094] Step S2. Assembly and debugging before welding: clamp the uncoated alumina ceramic base material and the titanium alloy base material with a special welding fixture, and firmly contact the power electrode wire with the alumina ceramic base material and the titanium alloy base material to be welded, and then put the fixture and the power electrode wire into a vacuum diffusion heating furnace;

[0095] Step S3. Set the diffusion welding process parameters and power supply parameters: the heating rate is 10℃ / min, the temperature is raised to 850℃, and then a pressure of 5MPa is applied, and the temperature is kept for 2h without applying an electric field. After completion, the cooling rate is controlled to 5℃ / min, and after cooling to 400℃, the furnace is cooled to complete the diffusion connection of alumina ceramics and titanium alloy.

[0096] Performance Test:

[0097] The shear strength test was performed on the alumina ceramic and titanium alloy welded parts prepared in Examples 1 to 6 and Comparative Examples 1 to 5 to obtain the interface shear strength. The results are shown in Tables 1 and 2 below:

[0098] Table 1 Summary of relevant experimental parameters

[0099]

[0100] Table 2 Summary of shear strength test results

[0101]

[0102]

[0103] Data Analysis:

[0104] It can be seen from Tables 1 and 2 that the alumina ceramic and titanium alloy welded parts prepared by the welding method provided by the present invention have good mechanical properties and large shear strength. This is because the present invention successfully achieves high-quality connection between alumina ceramics and titanium alloys by electric field assisted diffusion connection, greatly reduces the connection temperature and connection time required for welding, and effectively solves the problems of low efficiency and high production cost of traditional diffusion welding. By pre-plating a metal layer on the surface of the alumina ceramic, the generation of an interface brittle Ti-Al-O ternary compound layer can be avoided, the mechanical properties of the diffusion welding joint can be improved, and a full solid solution joint with high mechanical properties is obtained, which significantly improves the service performance of the alumina ceramic and titanium alloy diffusion welding joint. In addition, the use of a pre-plating method can expand the applicability range of electric field assisted diffusion connection materials and effectively reduce the performance requirements for equipment. Finally, by adjusting the coating type, power supply parameters and temperature parameters, the interface diffusion layer type, thickness and distribution mode of the diffusion welding joint can be regulated, thereby improving the mechanical properties of the joint and minimizing the thermal damage behavior of the welding temperature to the material.

[0105] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0106] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An electric field assisted quick connection welding method for alumina ceramics and titanium alloys, It is characterized in that The following steps are involved: Step S1. Cleaning the sample before welding; Step S2. Ceramic surface coating: coating a metal layer on the surface of the alumina ceramic to be welded; Step S3. Assembly before welding; Step S4. Set the diffusion welding process parameters and power supply parameters: the heating rate is 5-15℃ / min, the temperature is raised to 700-900℃, and then kept warm for 1-2h at a pressure of 1-4MPa, and an electric field is applied at the same time. After completion, the cooling rate is controlled to 5-10℃ / min, and after cooling to 400℃, the furnace is cooled to complete the diffusion connection between the alumina ceramic and the titanium alloy.

2. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The steps of cleaning the sample before welding in step S1 are as follows: mechanically grinding and polishing the surfaces to be welded of the alumina ceramic base material and the titanium alloy base material to be welded, and then subjecting them to ultrasonic cleaning and then drying them for standby use.

3. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The metal layer in step S2 is any one of a Mo layer and a Nb layer.

4. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The coating method in step S2 is magnetron sputtering.

5. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The thickness of the metal layer in step S2 is 10-20 μm.

6. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The steps of pre-welding assembly in step S3 are as follows: clamp the alumina ceramic base material and the titanium alloy base material by a welding fixture, fasten the power electrode wire to the alumina ceramic base material and the titanium alloy base material, and then fix the fixture and the power electrode wire in a vacuum heating furnace.

7. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that In step S3, the two ends of the power electrode wire are respectively connected to the two ends of the alumina ceramic base material and the titanium alloy to be welded.

8. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The current density of the electric field in step S4 is 10-100 mA / mm 2 , the applied voltage is 400-1000V.

9. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The electric field is maintained for 10-20 minutes in step S4.

10. The electric field assisted quick connection welding method of alumina ceramic and titanium alloy according to claim 1, It is characterized in that The type of the electric field in step S4 is any one of direct current, alternating current and pulse current.

Citation Information

Cited By

  • Method for realizing low-temperature diffusion bonding of zirconium and alloy thereof under action of constant-current electric field

    CN119387795A

  • Method for preparing Sn58Bi / Cu welding joint with assistance of electric pulse

    CN120095255A

  • Diffusion welding method for aluminum oxide ceramic and titanium alloy and prepared composite board

    CN120362686A