Nondestructive welding method for foam metal

Ultrasonic welding technology solves the problem of insufficient bonding strength of nickel foam joints, and achieves high strength and durability of foam metal foam joints, ensuring the stability of battery performance and efficient use of materials.

CN118893296APending Publication Date: 2024-11-05CHANGDE LYRUN MATERIAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411285511.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Traditional foam nickel joints have uneven bonding strength, easy to fall off and affect the internal resistance of the battery through crimping or hammering, resulting in waste of costs and inconvenient application.

Method used

Ultrasonic welding method is used to use high-frequency vibration energy to overlap areas of foam metal materials, and a non-destructive welded joint is formed through friction heat and fusion, enhancing the overall strength and durability of the joint.

Benefits of technology

The high-strength bonding effect of foam metal joints in horizontal and vertical directions is achieved, ensuring that the joints are not easily pulled off or peeled off, reducing material losses and battery internal resistance, and meeting battery capacity fluctuations requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893296A_ABST
    Figure CN118893296A_ABST
Patent Text Reader

Abstract

The invention specifically discloses a foam metal lossless welding method which comprises the following steps: carrying out ultrasonic welding on an overlapping region of two sections of foam metal through high-frequency vibration energy generated by ultrasonic waves, so that the overlapping region of the two sections of foam metal generates friction heat and is fused, and further forming a foam metal joint, and lossless welding of the foam metal is achieved. According to the welding method, the two sections of foam metal to be welded are welded on the basis of ultrasonic waves, then the foam metal connector without damage welding is obtained, the high-strength bonding effect is provided in the horizontal direction, the stability of the foam metal connector in the plane is ensured, meanwhile, good combination can be achieved in the vertical direction, and the welding efficiency is improved. The overall strength and durability of the foam metal joint are effectively enhanced, and the welded foam metal joint has the advantage of being not prone to being pulled off or stripped in the horizontal direction and the vertical direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of battery material processing, and in particular relates to a method for non-destructive welding of foam metals. Background Art

[0002] Nickel foam is widely used in positive electrode filling materials of nickel-hydrogen, nickel-cadmium, nickel-zinc and other batteries due to its unique physical and chemical properties, such as multi-layer porous structure, high specific surface area and porosity. As a skeleton material, it plays a key role as a carrier of filling materials and current collector. In addition, nickel foam is also used in the fields of particle impurity filtration, catalytic reaction carrier, heat dissipation conduction, electromagnetic shielding and energy absorption. Therefore, the application field of nickel foam is very wide, and it occupies a dominant position in the battery industry.

[0003] However, in the production process of nickel foam, due to factors such as raw material length restrictions, appearance defect removal, and packaging and reel change, joint problems are inevitable. The traditional nickel foam joint is to press or hammer the nickel foam stack manually or by equipment through a mold. The bonding principle of the pressing and hammering method is mainly to increase the contact area of ​​the two materials by applying external pressure or impact force, and minimize the contact distance between them, thereby increasing the interaction opportunities between the molecules or microstructures of the materials. This increase in physical contact depends to a certain extent on the friction between the contact surfaces to initially maintain the stability of the joint. However, since the friction between the contact surfaces of the materials is essentially limited and mainly depends on the surface roughness and positive pressure, the bonding strength achieved in this way is relatively limited. In particular, in the vertical direction, due to factors such as gravity, vibration or external force, the joint is more susceptible to pull-off or peeling forces. At this time, relying solely on friction to maintain the stability of the bond is particularly insufficient. In addition, problems such as uneven material deformation, stress concentration or insufficient contact surface fit that may exist during the pressing and hammering process will further weaken the bonding strength of the joint, especially the load-bearing capacity in the vertical direction.

[0004] At the same time, the resistance of the joints of crimping or hammering is higher than that of nickel foam products. The increase in resistance at the joints will technically lead to the defect of excessive internal resistance of the battery during application, or even make it impossible to be applied to the battery. In terms of cost, it is reflected in the double waste of nickel foam and battery slurry by customers, and even the plates with joints are directly discarded.

[0005] Therefore, the traditional crimping or hammering methods have the defects of uneven bonding strength, easy detachment of the joints and influence on the internal resistance of the battery. In view of this, the present application provides a non-destructive welding method for foam metal. Summary of the invention

[0006] This application is made in view of the above technical problems. The purpose is to provide a foam metal non-destructive welding method for solving the technical problems existing in the existing crimping or hammering foam metal joints, for enhancing the overall strength and durability of the foam metal welded joints, and ensuring that the foam metal joints are not easily pulled off or peeled off in both the horizontal and vertical directions.

[0007] In order to solve the above technical problems, the present application provides a foam metal non-destructive welding method, the method comprising:

[0008] The overlapping areas of two sections of foam metal materials are ultrasonically welded by high-frequency vibration energy generated by ultrasound, so that the overlapping areas of the two sections of foam metal materials generate friction heat and fuse, thereby forming a foam metal joint and realizing non-destructive welding of the foam metal.

[0009] In the above-mentioned non-destructive welding method for foam metal, two sections of foam metal materials are ultrasonically welded based on the high-frequency vibration energy generated by ultrasound, thereby obtaining a non-destructively welded foam metal joint. Since ultrasonic welding converts the kinetic energy of the foam metal and the air in its pores into heat energy under static pressure (because there is a mass difference between the foam metal and the air, the two materials will reflect different vibration frequencies under the same high-frequency vibration of ultrasound, and then mutual friction will occur between the air and the foam metal material. The mutual friction realizes the conversion of kinetic energy into heat energy at the microscopic level), and the surface of the foam metal material at the microscopic level is rough. , the wall thickness is very thin, and it has a three-dimensional porous shape. Therefore, the foam metal ribs that are in local contact will also achieve contact, friction and deformation between the ribs due to the heat energy converted by ultrasonic vibration. The friction heat generated by the ultrasonic high-frequency vibration on the contact surface of the foam metal ribs and the diffusion and recrystallization of the metal atoms between the ribs can be achieved under the condition of extremely thin wall thickness of the foam metal, thereby realizing the conversion of kinetic energy into heat energy and deformation energy (deformation energy refers to the energy change involved when an object is deformed under the action of external force), and realizing the bonding of foam metal ribs and the fusion of nickel metal under microscopic conditions. Although no obvious melting phenomenon occurs, the local heating and plastic deformation caused by ultrasonic high-frequency vibration and friction promote the diffusion and recrystallization between foam metal atoms, thereby realizing the metallurgical bonding between foam metals in the solid state. Therefore, the welding method provided in the present application not only provides a high-strength bonding effect for the foam metal joint in the horizontal direction, ensuring the stability of the foam metal joint in the plane, but also enables the foam metal joint to achieve good bonding in the vertical direction, thereby effectively enhancing the overall strength and durability of the foam metal joint, making the welded foam metal joint not easy to be pulled off or peeled off in both the horizontal and vertical directions.

[0010] In some embodiments, an alignment fixture is used to align the two sections of foam metal material to form an overlapping area of ​​the two sections of foam metal material.

[0011] In some embodiments, the width of the overlapping region between the two sections of foam metal material is greater than 1 mm.

[0012] In some embodiments, the overlapping areas of two sections of foam metal materials are staggered welded by high-frequency vibration energy generated by ultrasound, so that the surface of the formed foam metal joint is staggered with a plurality of grooves and protrusions, and the top surface of the protrusion is flush with the surface of the foam metal material.

[0013] In some embodiments, a plurality of grooves and protrusions are evenly and alternately arranged on the surface of the foam metal joint.

[0014] In some embodiments, the ultrasonic wave is emitted by an ultrasonic welding machine, and the amplitude of the ultrasonic welding machine is 20-150 μm, the frequency is 20-100 kHz, and the pressure is 100-500N.

[0015] In some embodiments, the ultrasonic welding machine is equipped with a welding head that matches the overlapping area of ​​the two sections of foam metal material, and the width of the welding head is greater than or equal to 1 mm.

[0016] In some embodiments, the ultrasonic wave emitted by the ultrasonic welding machine welds the overlapping area of ​​the two sections of the foam metal material for a time period greater than or equal to 3 seconds.

[0017] In some embodiments, the method further includes: performing a qualification inspection on the formed foam metal joint.

[0018] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 It is a flow chart of a method for non-destructive welding of foam metal in some embodiments of the present application. DETAILED DESCRIPTION

[0021] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0022] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0023] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0024] The general inventive concept of the embodiment of the present application is to provide a non-destructive welding method for foam metal, by applying ultrasound to the foam metal material joint for ultrasonic welding, thereby obtaining a non-destructive welded foam metal joint. Since ultrasonic welding converts the kinetic energy of the foam metal and the air in its pores into heat energy under static pressure, the surface of the foam metal material under microscopic conditions is rough, and the wall thickness is very thin, and it has a three-dimensional porous morphology, so the foam metal ribs in local contact will also achieve contact, friction and deformation between the ribs due to the heat energy converted by ultrasonic vibration, and the friction heat generated by the high-frequency vibration of the ultrasonic wave on the contact surface of the foam metal ribs, and the diffusion and recrystallization of the metal atoms between the ribs can be achieved under the condition of the extremely thin wall thickness of the foam metal, thereby realizing the conversion of kinetic energy into heat energy and deformation energy, and realizing the bonding between the foam metal ribs and the fusion of nickel metal under microscopic conditions. Although no obvious melting phenomenon occurs, the local heating and plastic deformation caused by the high-frequency vibration of the ultrasonic wave and friction promote the diffusion and recrystallization between the foam metal atoms, thereby realizing the metallurgical bonding between the foam metals in the solid state. Therefore, the welding method provided in the present application not only provides a high-strength bonding effect for the foam metal joint in the horizontal direction, ensuring the stability of the foam metal joint in the plane, but also enables the foam metal joint to achieve good bonding in the vertical direction, thereby effectively enhancing the overall strength and durability of the foam metal joint, so that the welded foam metal joint is not easy to pull off or peel off in the horizontal and vertical directions. Moreover, under the premise of ensuring sufficient bonding strength of the foam metal joint, the non-destructive welding method can also effectively reduce the welding width of the overlapping area of ​​the two sections of foam metal materials. The welding width can be as low as 1 mm, which can not only reduce material loss, but also reduce the influence of the width of the joint on the battery capacity, thereby meeting the fluctuation range requirements of the battery nominal capacity and realizing the non-destructive utilization of the foam metal joint.

[0025] Based on the above general concept, reference Figure 1 As shown, Figure 1 A flow chart of a method for non-destructive welding of foam metal in some embodiments of the present application is shown. In the embodiments of the present application, the ultrasonic welding pattern of the ultrasonically welded foam metal product is obliquely staggered. In other embodiments, the ultrasonic welding pattern may also be vertically arranged, horizontally arranged, or other shapes, but it is necessary to ensure that the ultrasonic welding pattern is staggered.

[0026] The present application provides a method for non-destructive welding of foam metals, the method comprising:

[0027] The overlapping areas of two sections of foam metal are ultrasonically welded by high-frequency vibration energy generated by ultrasound, so that the overlapping areas of the two sections of foam metal generate friction heat and fuse, thereby forming a foam metal joint and realizing non-destructive welding of the foam metal.

[0028] In the above embodiment, the width of the overlapping area of ​​the two sections of foam metal is greater than 1 mm, that is, the range of the preset width value can be any value above 1 mm. Exemplarily, the preset width value can be 1 mm, 10 mm, 50 mm, etc., and any value above 1 mm.

[0029] In an optional embodiment of the present application, an alignment fixture is used to align the two sections of foam metal to form an overlapping area of ​​the two sections of foam metal.

[0030] In the above-mentioned embodiment, the alignment fixture is a device or fixture for aligning two sections of foam metal to be welded so that the two sections of foam metal form a common overlapping area, such as: selecting a base plate with a width equivalent to the foam metal to be welded, and setting fixed side plates in parallel on both sides of the base plate to limit the width of the foam metal, thereby ensuring that the two sections of foam metal can be aligned. In other embodiments, alignment fixtures of other structures can also be selected, as long as it is ensured that the two sections of foam metal can be aligned and form a common overlapping area.

[0031] In the above implementation, the two sections of foam metal are aligned based on the alignment fixture, which provides a guarantee for the quality of the foam metal joint after subsequent ultrasonic welding.

[0032] In an optional embodiment of the present application, the overlapping areas of two sections of foam metal are alternately welded by high-frequency vibration energy generated by ultrasound, so that the surface of the formed foam metal joint is alternately provided with a number of grooves and protrusions, and the top surface of the protrusion is flush with the surface of the foam metal.

[0033] In the above embodiment, the high-frequency vibration energy generated by the ultrasonic wave is used to perform ultrasonic welding alternately on the overlapping areas of the two sections of foam metal, that is, ultrasonic welding is performed at intervals on the overlapping areas of the two sections of foam metal. The surface of the foam metal joint formed in this way will show a staggered distribution of grooves and protrusions. The position of the foam metal joint is formed with grooves after ultrasonic welding, while the area that has not been ultrasonically welded remains consistent with the original foam metal surface, thereby ensuring that the foam metal joint will not have abnormal equipment tooth jumping during actual use.

[0034] In the above embodiment, the plurality of grooves and protrusions on the surface of the foam metal joint are evenly and staggeredly arranged. This structure not only has a beautiful and neat appearance, but also makes the ultrasonic welding process easy to control.

[0035] In the above embodiment, the ultrasonic wave is emitted by an ultrasonic welding machine, and the amplitude of the ultrasonic welding machine is 20-150 μm, the frequency is 20-100 kHz, and the pressure is 100-500 N.

[0036] In the above embodiment, the ultrasonic welding machine is equipped with a welding head that matches the overlapping area of ​​the two sections of foam metal, and the width of the welding head is greater than or equal to 1 mm. The shape of the welding head can be selected based on actual conditions, and the width of the welding head should match the width of the overlapping area of ​​the two sections of foam metal, that is, the width of the welding head can be selected to be 1 mm, 10 mm, 50 mm, etc., and any value above 1 mm.

[0037] The welding time of the ultrasonic waves emitted by the ultrasonic welding machine on the overlapping area of ​​the two sections of foam metal is greater than or equal to 3s. Exemplarily, the welding time can be selected as 3s, 4s, 5s, 6s, 7s, etc., and any value greater than 3s.

[0038] In an optional implementation manner of the present application, the method further includes: performing a qualification inspection on the formed foam metal joint.

[0039] In the above implementation manner, the foam metal joint is subjected to a qualification inspection to confirm whether it meets the quality standard, thereby ensuring the quality of the ultrasonically welded foam metal joint product.

[0040] In order to better illustrate the working principle and beneficial effects of the technical solution of the present application, the performance of the foam metal product without joints, the crimped foam metal product with joints and the ultrasonic welded foam metal product are respectively tested. The performance test items include tensile strength test, resistance test and winding number test.

[0041] (I) The process of tensile strength test is as follows:

[0042] When cutting the test sample of the foam metal product with joints (the specifications of the foam metal product without joints are the same as those of the foam metal product with joints), place the joint position of the foam metal product in the middle of the sample to be tested, open the AnyTest test software (this test software is prior art and will not be described here), set the gauge length of the testing equipment (the testing equipment is a commercially available equipment for tensile strength testing) to 100mm, the sample size to 20mm*150mm, the test speed to 100mm / min, and the test data results are shown in Table 1, where the unit of the tensile strength test data is N / 20mm*100mm.

[0043] Table 1 Comparison of tensile strength test data

[0044]

[0045]

[0046] It can be seen from Table 1 that the tensile strength value of the ultrasonically welded foam metal product connected by ultrasonic welding in the present application is basically equivalent to the tensile strength value of the foam metal product without a joint, while the tensile strength value of the crimped foam metal product connected by traditional crimping is lower than the tensile strength value of the foam metal product without a joint. Therefore, the ultrasonically welded foam metal product connected by the non-destructive welding method provided in the present application effectively enhances the overall strength and durability of the welded joint of the foam metal product, and the welded foam metal joint is not easy to pull off or peel off in both the horizontal and vertical directions.

[0047] (II) The specific process of resistance testing is as follows:

[0048] When cutting the sample of the foam metal product, the joint position of the foam metal product is placed in the middle of the sample to be tested. The measuring instrument is a DC bridge resistance measuring instrument with a measuring length of 100mm. The size of the foam metal product sample is 100mm*150mm. The test data results are shown in Table 2. The unit of the resistance test data is mΩ / 10mm*100mm.

[0049] Table 2 Resistance test data comparison table

[0050]

[0051] It can be seen from Table 2 that the resistance value of the ultrasonically welded foam metal product connected by ultrasonic welding in the present application is basically equivalent to the resistance value of the foam metal product without a joint, while the resistance value of the crimped foam metal product connected by traditional crimping is greater than the resistance value of the foam metal product without a joint. Therefore, the resistance of the ultrasonically welded foam metal product connected by the non-destructive welding method provided in the present application is not affected, and therefore will not affect the internal resistance of the battery in the application.

[0052] (III) The specific process of winding number test is as follows:

[0053] 1) Cut the sample of the foam metal product. When cutting the sample of the foam metal product, place the joint of the foam metal product in the middle of the sample to be tested, and ensure that the winding test section includes the joint part. The size of the foam metal product sample is 20mm*150mm, and the specification of the foam metal product sample is 350g / m2;

[0054] 2) Clamp the test sample between the hyperbolic steel rod and fix it with the screws next to it;

[0055] 3) Put on the finger cot and wrap your index finger around the hyperbolic steel rod once, and then wrap it around in the opposite direction once;

[0056] 4) Until cracks larger than 1-2 mm visible to the naked eye appear at the joint or foam metal, and record the number and crack position.

[0057] The specific results of the winding number test are shown in Table 3.

[0058] Table 3 Comparison of winding times test data

[0059]

[0060] It can be seen from Table 3 that the winding times test value of the ultrasonic welded foam metal product connected by the ultrasonic welding method of the present application is basically equivalent to the winding times test value of the foam metal product without joints, and at the same time, the disconnection position of the winding test of the ultrasonic welded foam metal product connected by the ultrasonic welding method of the present application is not at the welding joint; while the winding times of the crimped foam metal product connected by the traditional crimping method is not only less than the winding times of the ultrasonic welded foam metal product, but also the disconnection position of the winding test of the crimped foam metal product is at the joint. Therefore, the overall strength and durability of the ultrasonic welded foam metal product connected by the non-destructive welding method provided by the present application are both superior to those of the crimped foam metal product, and the overall strength and durability of the ultrasonic welded foam metal product are equivalent to those of the foam metal product without joints.

[0061] The above is a detailed introduction to a foam metal non-destructive welding method provided by the present application. This article uses specific examples to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the core idea of ​​the present application. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.

Claims

1. A foam metal non-destructive welding method, characterized in that: The method comprises: The overlapping areas of two sections of foam metal materials are ultrasonically welded by high-frequency vibration energy generated by ultrasound, so that the overlapping areas of the two sections of foam metal materials generate friction heat and fuse, thereby forming a foam metal joint and realizing non-destructive welding of the foam metal.

2. The method for non-destructive welding of foamed metal according to claim 1, characterized in that: An alignment fixture is used to align the two sections of foam metal material to form an overlapping area of ​​the two sections of foam metal material.

3. The foam metal non-destructive welding method according to claim 2, characterized in that: The width of the overlapping area of ​​the two sections of foam metal material is greater than 1 mm.

4. The method for non-destructive welding of foamed metal according to claim 3, characterized in that: The overlapping areas of two sections of foam metal materials are staggered welded by high-frequency vibration energy generated by ultrasound, so that the surface of the formed foam metal joint is staggered with a plurality of grooves and protrusions, and the top surface of the protrusion is flush with the surface of the foam metal material.

5. The foam metal non-destructive welding method according to claim 4, characterized in that: A plurality of grooves and protrusions are evenly and staggeredly arranged on the surface of the foam metal joint.

6. The foam metal non-destructive welding method according to claim 5, characterized in that: The ultrasonic wave is emitted by an ultrasonic welding machine, and the amplitude of the ultrasonic welding machine is 20-150 μm, the frequency is 20-100 kHz, and the pressure is 100-500N.

7. The method for non-destructive welding of foamed metal according to claim 6, characterized in that: The ultrasonic welding machine is equipped with a welding head that matches the overlapping area of ​​the two sections of foam metal material, and the width of the welding head is greater than or equal to 1 mm.

8. The method for non-destructive welding of foamed metal according to claim 7, characterized in that: The ultrasonic wave emitted by the ultrasonic welding machine welds the overlapping area of ​​the two sections of foam metal material for a time greater than or equal to 3 seconds.

9. The foam metal non-destructive welding method according to claim 1, characterized in that: Also includes: The formed foam metal joint is inspected for quality.

Citation Information

Patent Citations

  • A method for using nickel foam connectors in nickel-metal hydride batteries

    CN102280644A

  • Power storage module

    CN109196684A

  • Tab welding method and battery prepared by tab welding method

    CN111375882A

  • Connecting method of three-dimensional porous member and method of manufacturing electrode